Charcoal Finery Iron: the South Wales Process, Ball Hammered into Stamps (Percy, 1864)
Forge

Dibuat oleh

Forge

4. November 2026NO
9
0
0
0
0

Charcoal Finery Iron: the South Wales Process, Ball Hammered into Stamps (Percy, 1864)

The best iron for charcoal tin-plates, as Percy watched it made at the Morfa Tin-plate Works, Llanelly, on 9 September 1859: pig iron melted under coke in a running-out fire flows into two charcoal fineries, where it is broken up with charcoal, melted down before a cold blast and worked into a ball, which is hammered into a slab and broken into 'stamps'. Charcoal is used because it holds no sulphide of iron, so no sulphur passes into the iron. Source: J. Percy, Metallurgy: Iron and Steel (1864), pp. 581-586. Picture: Fig. 107, the refinery and two charcoal fineries at Morfa.
Lanjutan
Unknown

Instruksi

1

Melt the pig under coke

Melt Pembrokeshire pig iron and Cumberland haematite pig iron together under coke in the running-out fire (melting finery), enough to fill two charcoal fineries: 5 to 6 cwt at Pont-y-Mister; 200 to 250 lb for each finery at Pontypool. Tap it at the bottom so that metal flows first, and keep the slag apart as far as you can. Not given: the proportion of the two pigs.

Material untuk langkah ini:

Batangan besi kasarBatangan besi kasar1 5-6 cwt for two fineries
Kokas metalurgiKokas metalurgi1 buah

Alat yang dibutuhkan:

Tungku pemurnian kokasTungku pemurnian kokas
Mesin peniupMesin peniup
2

Fill the charcoal fineries

Run the molten metal into the two charcoal fineries, still hot from the last heat. Take off the slag that comes with it as a crust once it has set. Throw in a basket of charcoal and let the cold blast on full.

Material untuk langkah ini:

Arang bongkah (kayu keras)Arang bongkah (kayu keras)1 a basket per finery, more as needed

Alat yang dibutuhkan:

Tungku pemurnianTungku pemurnian
Mesin peniupMesin peniup
3

Break up and melt down

Break the friable, half-set metal with an iron bar, mix it with the charcoal and heap it towards the tuyere side, where it melts down before the blast ('sinking a lump'). Throw water on the charcoal at intervals so that it does not burn to waste. Keep loosening and raising the metal from the bottom and the tuyere side.

Alat yang dibutuhkan:

Pengorek apiPengorek api
Tungku pemurnianTungku pemurnian
AirAir
4

Gather the ball

Put back pieces left from the last hammering with a two-pronged fork. Tap off the cinder several times and add charcoal, using the hooks at the sides as fulcra to press loose pieces down onto the ball. Lessen the blast at the end. At Morfa the metal went in at 2 h 10 m and the ball came out at 3 h 23 m.

Alat yang dibutuhkan:

Pengorek apiPengorek api
Tungku pemurnianTungku pemurnian
5

Hammer the ball into a slab

Put the ball under the cam hammer with the tuyere mark facing the hammerman. Hammer it into a narrow slab, rounded at the ends, about 1 3/4 to 2 1/4 in. thick. While it is hot, nick it across deeply in seven or eight places with a chisel-ended bar under the hammer.

Alat yang dibutuhkan:

Palu tempa nokPalu tempa nok
Penjepit TempaPenjepit Tempa
6

Quench and break into stamps

Plunge the nicked slab, still red-hot, into cold water to loosen the oxide. Lay it nicks down across a long ribbed anvil and break it with a narrow-ended sledge into 'stamps' of about 26 lb. Set the end pieces apart, sort the rest by soundness, and return broken bits to the next charge.

Alat yang dibutuhkan:

AirAir
Paron rataParon rata
GodamGodam
Penjepit TempaPenjepit Tempa

Bahan

3

Alat yang Diperlukan

9

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...