Clear Porcelain Glaze: Feldspar, Whiting, Kaolin and Flint, Binns 1910
Clay

Dibuat oleh

Clay

18. Oktober 2026DK
7
0
0
0
0

Clear Porcelain Glaze: Feldspar, Whiting, Kaolin and Flint, Binns 1910

Charles Binns's simplest porcelain glaze (The Potter's Craft, 1910): feldspar 167, whiting 70, kaolin 52 and flint 108 parts, ground fine with water. It fires clear and bright on porcelain at cone 10 to 12 in a reducing fire, and Binns says the same glaze also serves for stoneware. The picture: a Korean porcelain bottle under clear glaze, Joseon dynasty, c. 1400–1500 (Asian Art Museum, San Francisco; photo by Daderot, Wikimedia Commons, public domain).
Menengah
1 day

Instruksi

1

Powder the feldspar and flint

Pound the feldspar and the quartz sand to powder in the mortar and sift it through the fine sieve. Flint here means silica: Binns uses ground quartz or flint.

Material untuk langkah ini:

Bongkahan feldsparBongkahan feldspar167 g
Pasir KuarsaPasir Kuarsa108 g

Alat yang dibutuhkan:

Lumpang dan AluLumpang dan Alu
Ayakan Jaring HalusAyakan Jaring Halus
2

Weigh the batch

Weigh in grams: feldspar 167, whiting 70, kaolin 52, flint 108.

Material untuk langkah ini:

Kalsium karbonat (kapur tulis halus)Kalsium karbonat (kapur tulis halus)70 g
Bubuk lempung kaolinBubuk lempung kaolin52 g

Alat yang dibutuhkan:

Neraca lenganNeraca lengan
3

Grind with water

Grind the batch with half a pint of water. Binns grinds about an hour in a ball mill; by hand in a mortar works too, with fine sieves.

Material untuk langkah ini:

AirAir250 ml

Alat yang dibutuhkan:

Lumpang dan AluLumpang dan Alu
4

Sieve and settle

Rinse everything out with plenty of water and keep the washings. Strain through a 120-mesh sieve, let it settle, and pour off the clear water.

Alat yang dibutuhkan:

Ayakan Jaring HalusAyakan Jaring Halus
EmberEmber
5

Thick as cream

Use it as thick as cream: a dipped finger comes out with a white coat that will not shake off.

Alat yang dibutuhkan:

EmberEmber

Bahan

5

Alat yang Diperlukan

4

Cetak biru ini membuat

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.