Flat-Bit Tongs and the Tongs Made from Them, down to Crucible Tongs: Welded Reins, Riveted Joint (Edwinson, 1886)
Forge

Dibuat oleh

Forge

14. November 2026NO
10
0
0
0
0

Flat-Bit Tongs and the Tongs Made from Them, down to Crucible Tongs: Welded Reins, Riveted Joint (Edwinson, 1886)

George Edwinson's tong-making lesson from Amateur Work (1886): jaws forged from inch-square iron, reins of 5/8 in. rod scarfed and welded on, the halves riveted with a hot iron pin. The same flat-bit tongs are then reshaped into pincer, hammer and crook-bit tongs, light smith's pliers, and thinned and curved into crucible tongs.
Lanjutan
A day at the forge

Instruksi

1

His sizes

Memuat notebook Jupyter…
2

Read Edwinson

"Indeed, the man who can turn out a good pair of tongs may be trusted with almost any job in the smithy."
3

Forge the reins

Cut two pieces of 5/8 in. (16 mm) iron rod, each 2 ft (0.6 m) long, with a cold chisel. Bring one end of each to a white welding heat and draw 3-4 in. down to a taper from 5/8 to 1/2 in., rounded for the hand. Upset the other ends at a white heat and scarf them (his figs. 27-28).

Material untuk langkah ini:

Batang besi tempaBatang besi tempa1 buah

Alat yang dibutuhkan:

Pahat besi dinginPahat besi dingin
Perapian pandai besiPerapian pandai besi
Landasan TempaLandasan Tempa
PaluPalu
Tang pandai besiTang pandai besi
4

Forge the jaws

Cut two 6 in. pieces of 1 in. square iron (or one 12 in. bar, worked from each end before cutting, fig. 29). Forge each jaw end 4 in. long, 1 1/4 in. wide and 3/8 in. thick. Flatten the other end to 1/4 in. thick, round it for the joint (fig. 30) and draw it to a slightly rounded taper (fig. 31).

Material untuk langkah ini:

Batang persegi baja lunakBatang persegi baja lunak1 buah

Alat yang dibutuhkan:

Perapian pandai besiPerapian pandai besi
Landasan TempaLandasan Tempa
PaluPalu
Tang pandai besiTang pandai besi
5

Punch the joint

Mark the hole with a centre punch, heat, and punch a 3/8 in. hole over the anvil's heel hole with an iron punch tapering 1/4 to 1/2 in. (fig. 35), or a steel punch of 5/8 in. tool steel.

Material untuk langkah ini:

Batang baja perkakasBatang baja perkakas1 buah

Alat yang dibutuhkan:

PenitikPenitik
Perapian pandai besiPerapian pandai besi
Landasan TempaLandasan Tempa
PaluPalu
6

Weld jaw to rein

Scarf the taper end of each jaw to fit a rein. Heat both to a welding heat in a clear fire, throw on clean fine fresh-water sand and heat until pasty. Tap the scarfs together lightly, return to the fire a moment, and finish the weld. At a red heat forge the square part to blend into the round rein (fig. 32).

Material untuk langkah ini:

PasirPasir1 buah

Alat yang dibutuhkan:

Perapian pandai besiPerapian pandai besi
Landasan TempaLandasan Tempa
PaluPalu
Tang pandai besiTang pandai besi
7

Rivet the joint

Smiths' way: nick a 3/8 in. round iron rod to rivet length, put the halves together, insert the hot end, twist it off, let 1/4 in. stand below, and rivet both sides. (Or make a 3/4 x 3/8 in. button-headed rivet in a 3/8 in. hole in a flat iron.) If the joint locks, reheat jaws and pin to bright red and work them free.

Material untuk langkah ini:

Batang besi tempaBatang besi tempa1 buah

Alat yang dibutuhkan:

Perapian pandai besiPerapian pandai besi
Landasan TempaLandasan Tempa
PaluPalu
Landasan kepala pakuLandasan kepala paku
8

Set the jaws

Heat the jaws and set them to the width of the stock to be held. Spring them wider with a piece of cold iron between and a few light blows.

Alat yang dibutuhkan:

Perapian pandai besiPerapian pandai besi
Landasan TempaLandasan Tempa
PaluPalu
9

Crucible tongs and other forms

From flat-bit tongs at the fig. 32 stage: lengthen and curve the bits for pincer tongs (angular notches hold round or square bars), more for hammer tongs, bend them sideways for crook-bit tongs. Small flat-bit tongs with lengthened, shaped bits are smith's pliers; thin those out further and curve them like pincers to make crucible tongs for hot crucibles and pots of molten metal. Heavy tongs 2-5 ft long need stouter iron.

Alat yang dibutuhkan:

Perapian pandai besiPerapian pandai besi
Landasan TempaLandasan Tempa
PaluPalu
Tang pandai besiTang pandai besi
10

Troubleshooting

Tongs troubleshooting.

Flow

Loading...
11

History and honest limits

From George Edwinson, "Smithing and Forging" III, **Amateur Work, Illustrated**, vol. V (1886), pp. 266-269 (checked on the archive.org scan amateurworkillus05lond). He gives full sizes only for the flat-bit tongs; crucible tong sizes and curvature are left to the work. Metric figures and tools are ours.

Bahan

4

Alat yang Diperlukan

7

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...