Smith's Fire Rake (Poker): a 3/8 in. Rod Drawn to a Flat Point, Crooked, and Looped Over the Anvil (Edwinson, 1886)
The first job George Edwinson set his readers in Amateur Work (1886): the smith's rake for the forge fire, which "might be dubbed a poker". A yard of 3/8 in. iron rod drawn to a square then flat point with quarter turns, bent into a crook, and the other end bent round in three heats into a loop handle.
Pemula
An hour at the forge
Instruksi
1
1
His sizes
His sizes
Memuat notebook Jupyter…
2
2
Read Edwinson
Read Edwinson
"The rake, Fig. 16, might be dubbed a poker, and as this is the most simple tool, we will deal with that first."
3
3
Light a small fire
Light a small fire
Pile slack round the tuyere, scoop a shallow pit in front of it, put in shavings with a few cinders on top, light and blow gently. Draw slack in until the heap glows, then damp the outside so the fire stays within 6 in. (15 cm) of the tuyere.
Material untuk langkah ini:
Batu bara bituminus1 buahAlat yang dibutuhkan:
Perapian pandai besi4
4
Draw the point
Draw the point
Cut 36 in. (91 cm) of 3/8 in. (10 mm) iron rod with a cold chisel. Heat 2 in. of one end glowing white. On the outer edge of the anvil, hammer it lightly on the tip, giving the rod a quarter turn after each blow and drawing it back, to a square point. Strike only while it glows; reheat at a dull red. Next heat, round the corners and draw a flat tapering point (fig. 17).
Material untuk langkah ini:
Batang besi tempa1 buahAlat yang dibutuhkan:
Pahat besi dingin
Perapian pandai besi
Landasan Tempa
Palu5
5
Crook the end
Crook the end
Heat the point to a dull red and bend it over the outer edge of the anvil with a few light blows into the crook (fig. 16).
Alat yang dibutuhkan:
Perapian pandai besi
Landasan Tempa
Palu6
6
Bend the loop
Bend the loop
Heat the rod about 10 in. from the other end to redness and bend it over the anvil edge (fig. 18). Heat 3 in. more of the bent part and shape it (fig. 19). Heat again and bring the end round to touch the shoulder (fig. 20), then shape the loop hot with light blows. (Experienced smiths scarf the end and weld it to the shoulder.)
Alat yang dibutuhkan:
Perapian pandai besi
Landasan Tempa
Palu7
7
Troubleshooting
Troubleshooting
Rake troubleshooting.
Flow
Loading...
8
8
History and honest limits
History and honest limits
From George Edwinson, "Smithing and Forging" II, **Amateur Work, Illustrated**, vol. V (1886), pp. 211-213 and figs. 15-20 (checked on the archive.org scan amateurworkillus05lond). Metric figures and the tools are ours.
Bahan
2- 1 buahPlaceholder
- 1 buahPlaceholder
Cetak biru ini membuat
Blueprint terkait
Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip
CC0 Domain Publik
Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.
Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.