Electrolytic Iron: Brown Ferrous Electrolyte, Rotating Cathode at 75-77 °C, Graphite Anodes (Bouchayer, US 1,516,326)
Charlie

Dibuat oleh

Charlie

31. Oktober 2026DE
0
0
0
0
0

Electrolytic Iron: Brown Ferrous Electrolyte, Rotating Cathode at 75-77 °C, Graphite Anodes (Bouchayer, US 1,516,326)

Iron plated out of a fresh green ferrous bath comes off rough and useless. Bouchayer first stirred the bath in air until it turned bright brown; the iron oxychloride formed takes care of the hydrogen at the cathode, and the deposit grows even and compact at high current. Result: electrolytic iron, deposited at about 98 % current yield. Source: Bouchayer, US 1,516,326 (1924). Not given: cathode material, purity of the iron. Picture drawn by Youblob.
Lanjutan
Factory process

Instruksi

1

Make up the electrolyte at 20 °Bé

Dissolve ferrous sulfate in water (Bouchayer also allows ferrous chloride or a mix). Concentration: e.g. 20 °Bé, then keep it constant.

Material untuk langkah ini:

Besi sulfatBesi sulfat1 as required

Alat yang dibutuhkan:

AirAir
HidrometerHidrometer
Bak elektrolisisBak elektrolisis
2

Stir it in air until brown

Agitate the green bath in air, e.g. by turning the anode, until it is bright brown and stops foaming. Used green, it gives only an irregular deposit.

Alat yang dibutuhkan:

Bak elektrolisisBak elektrolisis
3

Circulate it through iron filings

Pump the electrolyte through a mass of iron filings in a separate vessel; it takes back iron and forms the ferric hydroxide that keeps the bath working. Keep it moving fast past the anodes: this lowers the phosphorus.

Material untuk langkah ini:

Serbuk besiSerbuk besi1 as required

Alat yang dibutuhkan:

Pompa airPompa air
4

Deposit on a rotating cathode

Electrolyse between graphite anodes and a rotating cathode. Temperature: e.g. 75-77 °C at 1000 A/m², held exactly constant and below boiling; cathode speed: e.g. 120 m/min at 800 A/m². Cathode material: not given.

Alat yang dibutuhkan:

Elektrode grafitElektrode grafit
Sumber daya arus searahSumber daya arus searah
TermometerTermometer
Bak elektrolisisBak elektrolisis
5

Strip and reheat the deposit

Take the compact iron deposit off the cathode; it is usable after a slight reheating (temperature not given).

Alat yang dibutuhkan:

Bak elektrolisisBak elektrolisis

Bahan

2
  • 1 as required
    Placeholder
  • 1 as required
    Placeholder

Alat yang Diperlukan

7

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...