Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 50 °C (McIntire, Dow 1948, Ex. 3, Test 2)

Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 50 °C (250 psi in the tower), it swelled into a log 6 to 9 inches across, weighing 4.8 lb per cubic foot, with somewhat smaller, uniform cells. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
Lanjutan
3 days

Instruksi

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Material untuk langkah ini:

PolistirenaPolistirena300 pon

Alat yang dibutuhkan:

Reaktor bertekananReaktor bertekanan
Neraca lenganNeraca lengan
Sarung tangan karetSarung tangan karet
2

Add the propylene fraction

Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.

Material untuk langkah ini:

PropilenaPropilena100 pon

Alat yang dibutuhkan:

Tabung gas bertekananTabung gas bertekanan
Reaktor bertekananReaktor bertekanan
Kacamata Pelindung Cipratan KimiaKacamata Pelindung Cipratan Kimia
3

Stand two days at 40 °C

Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.

Alat yang dibutuhkan:

Reaktor bertekananReaktor bertekanan
Termometer LaboratoriumTermometer Laboratorium
4

Let it out at 50 °C

Open the valved outlet near the bottom (3.25 inch in the patent) at 50 °C. The pressure is about 250 psi. The gel flows out and swells into a log 6 to 9 inches across, 4.8 lb per cubic foot, with somewhat smaller, uniform cells. Close the outlet again. The patent heated step by step (50, 60, 75 °C) for several hours each, letting a portion out at each step.

Alat yang dibutuhkan:

Reaktor bertekananReaktor bertekanan
Termometer LaboratoriumTermometer Laboratorium
Kacamata Pelindung Cipratan KimiaKacamata Pelindung Cipratan Kimia
Sarung tangan karetSarung tangan karet
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Alat yang dibutuhkan:

Gergaji tukang kayuGergaji tukang kayu
Sarung tangan karetSarung tangan karet

Bahan

2
  • Placeholder
  • 100 pon
    Placeholder

Alat yang Diperlukan

7

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...