Ferrite Toroid Core: Copper-Zinc Ferrite Sintered at 1250 °C, Presintered Three Times at 900 °C (Snoek 1948, Ex. I)
A soft ferrite ring core for coils and transformers: copper, zinc and iron oxides with a little brownstone, presintered three times at 900 °C, pressed into a ring and sintered at 1250 °C in oxygen. Snoek's ring had an initial permeability of 1,580. Its Curie point was about 80 °C.
Source: J. L. Snoek, US 2,452,530 (Philips, 1948), Example I and its table. Unknown: the 'violet' iron oxide, linked to an unknown head. Picture: the patent's Fig. 4, the ring core.
Lanjutan
2 days
Instruksi
1
1
Weigh 20 : 30 : 50 mol % and 1 % brownstone
Weigh 20 : 30 : 50 mol % and 1 % brownstone
Mix 20 mol % pure copper oxide, 30 mol % pure zinc oxide and 50 mol % pure violet iron oxide, and add 1 % by weight of brownstone (manganese dioxide). Ours, by weight: 13.24 g copper oxide, 20.32 g zinc oxide and 66.44 g iron oxide per 100 g, plus 1 g brownstone. Unknown: what makes the iron oxide 'violet'; Snoek does not say.
Material untuk langkah ini:
Tembaga Oksida13.24 g
Serbuk Seng Oksida20.32 g
Oksida besi ungu66.44 g
Mangan dioksida (pirolusit)1 gAlat yang dibutuhkan:
Neraca lengan
Masker Debu2
2
Grind half an hour in an iron ball mill
Grind half an hour in an iron ball mill
Grind the mixture for half an hour in a mill with iron balls.
Alat yang dibutuhkan:
Ball Mill Besi
Masker Debu3
3
Presinter at 900 °C for 2 hours in oxygen
Presinter at 900 °C for 2 hours in oxygen
Heat the ground powder to 900 °C for 2 hours in oxygen and let it cool.
Alat yang dibutuhkan:
Tungku Tabung
Oksigen
Tabung gas bertekanan
Pirometer
Krus dengan tutup (porselen)
Sarung Tangan Tahan Panas4
4
Grind and presinter at 900 °C again (2 of 3)
Grind and presinter at 900 °C again (2 of 3)
Grind the powder, then heat it once more to 900 °C in oxygen. Snoek gives no times for the repeats.
Alat yang dibutuhkan:
Ball Mill Besi
Tungku Tabung
Oksigen
Tabung gas bertekanan
Krus dengan tutup (porselen)
Sarung Tangan Tahan Panas
Masker Debu5
5
Grind and presinter at 900 °C again (3 of 3)
Grind and presinter at 900 °C again (3 of 3)
Grind the powder, then heat it once more to 900 °C in oxygen. Snoek gives no times for the repeats.
Alat yang dibutuhkan:
Ball Mill Besi
Tungku Tabung
Oksigen
Tabung gas bertekanan
Krus dengan tutup (porselen)
Sarung Tangan Tahan Panas
Masker Debu6
6
Grind 2 hours with iron balls
Grind 2 hours with iron balls
Grind it for 2 hours in a disintegrator with iron balls.
Alat yang dibutuhkan:
Ball Mill Besi
Masker Debu7
7
Press a ring at 4 tons per cm²
Press a ring at 4 tons per cm²
Press the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm cross-section.
Alat yang dibutuhkan:
Mesin pres hidrolik
Cetakan Penekan Cincin
Masker Debu8
8
Sinter at 1250 °C in oxygen, cool 5–10 °C a minute
Sinter at 1250 °C in oxygen, cool 5–10 °C a minute
Sinter the ring at 1250 °C in a current of oxygen. Example I heats for 1 hour and cools in the oxygen at 5 to 10 °C per minute. Snoek's ring had an initial permeability of 1,580, measured at room temperature at 2 kHz.
Alat yang dibutuhkan:
Tungku Tabung
Oksigen
Tabung gas bertekanan
Pirometer
Penjepit Kowi
Sarung Tangan Tahan PanasBahan
4- 13.24 gPlaceholder
- 20.32 gPlaceholder
- 66.44 gPlaceholder
- Placeholder
Alat yang Diperlukan
12- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Cetak biru ini membuat
Blueprint terkait
Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip
CC0 Domain Publik
Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.
Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.