Fired Silver Paint: Silver Oxide and Flux in Polyvinyl Alcohol and Water (Gray, Erie Resistor 1954, Ex. 2)
Ed

Dibuat oleh

Ed

28. Oktober 2026FI
2
0
0
0
0

Fired Silver Paint: Silver Oxide and Flux in Polyvinyl Alcohol and Water (Gray, Erie Resistor 1954, Ex. 2)

A paint for putting silver electrodes on ceramic, glass or mica. Silver oxide and a little ceramic flux are held in polyvinyl alcohol dissolved in water. The wet paint conducts electricity, so a capacitor can be measured while it is being painted. On firing, the silver oxide turns into a silver film held on by the flux. Gray found this paint so stable that it kept six months. Source: Robert B. Gray, US 2,695,275 (Erie Resistor, 1954), Example 2. Not given: which flux, and the firing heat. Bismuth subnitrate, one of the fluxes Gray names, is ours. Picture drawn by Youblob.
Pemula
1 day

Instruksi

1

Dissolve 2 g polyvinyl alcohol in the water

For 100 g of paint: dissolve 2 g polyvinyl alcohol in the water, warming it to help it dissolve. The water is the balance, about 34 to 44 g. Warming is ours.

Material untuk langkah ini:

Bubuk polivinil alkoholBubuk polivinil alkohol2 g
Air SulingAir Suling1 as required

Alat yang dibutuhkan:

Neraca lenganNeraca lengan
Gelas Piala BorosilikatGelas Piala Borosilikat
Pelat PemanasPelat Pemanas
Batang Kaca BorosilikatBatang Kaca Borosilikat
2

Grind in silver oxide and flux

Grind 50 g precipitated silver oxide and 2 to 10 g ceramic flux into the solution until smooth. Gray gives the flux only as a class; ours: bismuth subnitrate, one of the common fluxes he names. The right amount depends on the ceramic it will be fired onto.

Material untuk langkah ini:

Perak oksidaPerak oksida50 g
Bismut subnitratBismut subnitrat1 as required

Alat yang dibutuhkan:

Neraca lenganNeraca lengan
Lumpang dan AluLumpang dan Alu
Sarung Tangan NitrilSarung Tangan Nitril
3

Add 2 to 4 g alcohol against foam

Stir in 2 to 4 g ethyl alcohol. It stops the polyvinyl alcohol from foaming.

Material untuk langkah ini:

Etanol mutu laboratorium, 95 %Etanol mutu laboratorium, 95 %1 as required

Alat yang dibutuhkan:

Batang Kaca BorosilikatBatang Kaca Borosilikat
4

Store

Keep it in a closed jar. Gray found no reaction between the ingredients in six months, and the paint can stand for some hours in use without stirring.

Alat yang dibutuhkan:

Stoples Kaca Gelap Bertutup KedapStoples Kaca Gelap Bertutup Kedap

Bahan

5

Alat yang Diperlukan

7

Cetak biru ini membuat

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...