Glass Tube: Drawn by Two Glassmakers Walking Apart (Pellatt, 1849)
Charlie

Dibuat oleh

Charlie

4. November 2026DE
8
0
0
2
0

Glass Tube: Drawn by Two Glassmakers Walking Apart (Pellatt, 1849)

How glass tube was made by hand: a blown gather of glass is welded at one end to a second rod, and two workers walk away from each other while turning, stretching the hot glass into a tube up to 60 or 70 feet long. Because the whole bubble stretches evenly, the bore and the wall stay in the same proportion all along the tube. Result: long glass tube of nearly even bore, cut into lengths when cold. Solid cane is made the same way without blowing. Source: Apsley Pellatt, Curiosities of Glass Making (1849), pp. 106-108. Unknown: the glass batch and the gather's size. Picture: the book's figures.
Ahli
Unknown

Instruksi

1

Gather and blow the ball

Gather a solid ball of flint glass on the end of the blowing iron and blow it out a little, so it is hollow. When it has partly cooled, use it as a core for one or more further gatherings until there is enough glass. For flat-bore thermometer tube, flatten the first ball on the marver with an iron or wooden battledore before the later gatherings. Ours: lead crystal. Not given: the amount of glass.

Material untuk langkah ini:

Kristal timbalKristal timbal1 flint glass

Alat yang dibutuhkan:

Tanur kaca yang mampu mencapai 1100 derajat CelsiusTanur kaca yang mampu mencapai 1100 derajat Celsius
Pipa tiup peniup kacaPipa tiup peniup kaca
Marver (papan penggelinding kaca)Marver (papan penggelinding kaca)
2

Swing it long and fix the post

Lengthen the ball by swinging it, and chill its far end by dipping it in cold water. A second worker makes a disc of hot glass on a rod, the 'post', and holds it upright near the ground. The chief worker climbs onto a chair and drops the hot ball onto the post, where it welds on.

Alat yang dibutuhkan:

AirAir
Tongkat pontilTongkat pontil
3

Walk apart and draw

The chief worker steps down and the two walk away from each other, both turning their rods all the time. At first the hot glass sags between them in a curve; fan the parts that are thicker to cool them, so it stretches evenly. Draw it to the length wanted, up to 60 or 70 feet; as it cools it stops turning and pulls nearly straight. Except at the ends, it has nearly one bore, diameter and wall thickness. Ours: a wooden paddle for fanning (Pellatt: a boy's hat).

Alat yang dibutuhkan:

Pipa tiup peniup kacaPipa tiup peniup kaca
Tongkat pontilTongkat pontil
Pengaduk kayu bergagangPengaduk kayu bergagang
4

Lay down and cut

Lay the tube across the wooden rungs of a ladder to cool. Cut it into lengths by touching it with a cold iron or nicking it with a steel file.

Alat yang dibutuhkan:

Tangga kayuTangga kayu
Kikir LogamKikir Logam

Bahan

1
  • 1 flint glass
    Placeholder

Alat yang Diperlukan

8

Cetak biru ini membuat

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.