Forged Centre Punches and Pin Punches: Point Hardened in Brine, Temper Run to Straw from the Stock (Griswold, Amateur Work, 1904)
Robert Gibson Griswold's first tool-making lesson in Amateur Work (Boston, 1904): four centre punches from heavy to fine and nine pin, drift, offset and riveting punches, forged from carbon tool steel, finished with file and emery, then the point alone dipped in brine and the temper let run down from the hot stock to straw yellow.
Menengah
A day for the set
Instruksi
1
1
His sizes
His sizes
Memuat notebook Jupyter…
2
2
Read Griswold
Read Griswold
"The more work put into the steel at the working point the better will be its grade."
3
3
Forge the blanks
Forge the blanks
Forge carbon tool steel at no more than a bright red into the shapes of his fig. 2: a 3/8 in. chamfered head, a 2 1/2 in. body and a 1 1/2 in. taper. Heavy centre punch at least 5/8 in. across with a conical point about 3/8 in. at the base; lighter centre punches 3/8 and 1/4 in.; pin punches 1/2, 3/8 (square end), 5/16 and 1/4 in., plus parallel-ended, offset and round-ended ones.
Material untuk langkah ini:
Batang baja perkakas1 buahAlat yang dibutuhkan:
Perapian pandai besi
Landasan Tempa
Palu
Tang pandai besi4
4
Finish before hardening
Finish before hardening
Do all work except grinding the point now: file each punch to shape and finish it with emery cloth. Keep the striking head slightly rounded so it does not broom.
Material untuk langkah ini:
Kain emeri1 buahAlat yang dibutuhkan:
Kikir (Kikir Tangan)5
5
Harden the point
Harden the point
Heat the point to a dull red and plunge only the point, about 1/2 in. (13 mm), into a brine bath.
Material untuk langkah ini:
Larutan garam jenuh1 buahAlat yang dibutuhkan:
Perapian pandai besi
Tang pandai besi
Ember6
6
Run the temper
Run the temper
When the point is black, rub a bright spot with emery cloth on a flat stick and watch the heat from the stock colour it. At straw yellow (460 F) plunge the whole punch in water and keep it moving. If the stock has too little heat, lay it over the furnace to draw the colour.
Material untuk langkah ini:
Air1 buah
Kain emeri1 buahAlat yang dibutuhkan:
Ember
Perapian pandai besi7
7
Grind the points
Grind the points
Grind the points to shape after hardening without letting the edge turn blue; if it blues, grind back to hard metal.
Alat yang dibutuhkan:
Gerinda duduk8
8
Troubleshooting
Troubleshooting
Punch troubleshooting.
Flow
Loading...
9
9
History and honest limits
History and honest limits
From Robert Gibson Griswold, "Tool Making for Amateurs" I, **Amateur Work** (Boston), vol. III (1903-04), pp. 273-275 and fig. 2 (checked on the archive.org scan amateurwork03bostrich). Metric figures and tools are ours.
Bahan
4- 1 buahPlaceholder
- 2 buahPlaceholder
- 1 buahPlaceholder
- 1 buahPlaceholder
Cetak biru ini membuat
Blueprint terkait
Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip
CC0 Domain Publik
Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.
Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.