Black Cobbler's Wax: Resin and Pitch With Linseed Oil, Pulled to Golden Colour (Hasluck, Harness Making, 1904)
Forge

Dibuat oleh

Forge

14. November 2026NO
8
0
0
0
0

Black Cobbler's Wax: Resin and Pitch With Linseed Oil, Pulled to Golden Colour (Hasluck, Harness Making, 1904)

The saddler's black wax for waxed threads, from P. N. Hasluck's Harness Making (1904): half a pound each of resin and pitch melted together, softened with boiled linseed oil to suit the season, poured into cold water and pulled by wet hands until golden and until a piece floats. It makes about thirty lumps, kept under water.
Pemula
About 1 hour

Instruksi

1

Batch in grams

Memuat notebook Jupyter…
2

Read Harness Making

"Black cobbler's wax is made by melting together 1/2 lb. each of resin and pitch."
3

Melt and oil

Melt 1/2 lb of resin and 1/2 lb of pitch together and mix thoroughly. Take the pan off the fire and add boiled linseed oil, about a pennyworth or less: only half as much in summer as in winter, more the colder it is. Mix well.

Material untuk langkah ini:

Getah PinusGetah Pinus1 buah
Pek ter kayuPek ter kayu1 buah
Minyak Biji Rami MasakMinyak Biji Rami Masak1 buah

Alat yang dibutuhkan:

Panci BesarPanci Besar
Obor PropanaObor Propana
Neraca lenganNeraca lengan
4

Test

Pour a little into cold water, leave it a minute, and take it out with well-wetted hands. If it cracks when worked it is too hard; if it pulls out and sticks together it is right. Do not put the tested piece back in the pan: the water in it froths the hot wax.

Alat yang dibutuhkan:

Ember 20 LiterEmber 20 Liter
5

Pour and pull

Put the test piece back in the water and pour the rest in after it. Gather the wax with wet hands without delay and pull it fast, hand over hand, until it is a light golden colour. Cut off a piece with wet scissors and drop it in the water: if it floats it has been pulled enough; if it sinks, pull more. Under-pulled wax is brittle.

Alat yang dibutuhkan:

Ember 20 LiterEmber 20 Liter
GuntingGunting
6

Adjust and store

If it is too hard, melt again and add oil; if too soft, add pitch and resin. Cut it into lumps the size of a large pigeon's egg (about thirty) and keep them in water.

Alat yang dibutuhkan:

GuntingGunting
Ember 20 LiterEmber 20 Liter
7

Troubleshooting

Wax troubleshooting.

Flow

Loading...
8

History and honest limits

From Paul N. Hasluck, **Harness Making** (1904), "Harness-makers' Materials" (checked on the archive.org scan harnessmaking00hasl, pp. 30-31). He says only "pitch"; wood-tar pitch is our choice. His white wax, made with white lead, is left out because white lead is a poison. The metric figures and the diagram are ours.

Bahan

3

Alat yang Diperlukan

5

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...