High-Speed Steel, Charge 3: Crucible-Melted Tungsten-Chrome-Molybdenum-Vanadium Steel (Carnegie & Gladwyn 1918)
High-speed steel holds its edge when it is cutting hot. In Sheffield it was made like other crucible tool steel: the best Swedish bar iron melted in small clay pots in a coke fire, with tungsten, chromium, molybdenum and vanadium added to the liquid iron. This is the third of three typical charges given by Carnegie and Gladwyn: 55 lb iron, 26 lb tungsten powder, 12 lb ferro-chrome, 9.5 lb ferro-molybdenum and 1 lb ferro-vanadium for 100 lb of steel.
Source: D. Carnegie and S. C. Gladwyn, Liquid Steel (1918), pp. 74-77, 106-107 and 113. Unknown: how the Swedish iron, the tungsten powder, the ferro-molybdenum and the ferro-vanadium are made; the melting time; and how the ingot is worked into bar. The book stops at the liquid steel, so these are linked to unknown heads. Picture: the book's Fig. 29, crucible furnaces at Samuel Osborn & Co., Sheffield.
Ahli
1 day
Instruksi
1
1
Weigh charge 3
Weigh charge 3
For 100 lb of steel: 55 lb best Swedish bar iron, cut up; 26 lb tungsten powder (96 to 98 % tungsten); 12 lb ferro-chrome (60 % chromium); 9.5 lb ferro-molybdenum (80 % molybdenum); 1.0 lb ferro-vanadium (35 to 40 % vanadium). Unknown: how the Swedish iron, tungsten powder, ferro-molybdenum and ferro-vanadium are made. The book only lists them.
Material untuk langkah ini:
Besi batang Swedia55 pon
Serbuk tungsten26 pon
Ferokrom12 pon
Feromolibdenum9.5 pon
Ferovanadium1 ponAlat yang dibutuhkan:
Neraca lengan2
2
Set two clay crucibles in the melting hole
Set two clay crucibles in the melting hole
Tool steels are melted in small crucibles, about 55 lb each, two to a hole in a Huntsman coke furnace (ours: the 100 lb charge split between the two). Stand them on fireclay stands on the fire bars, straight from the annealing furnace, and fill the hole with coke up to their tops. Use the best washed coke, as free from sulphur as possible: sulphur gets into the steel even through the lid. When the pots are white hot, throw in a little sand to fuse them onto their stands.
Alat yang dibutuhkan:
Tungku krusibel
Kowi Tanah Liat Tahan Api
Kokas metalurgi
Pasir
Penjepit Kowi3
3
Melt the iron, then add the alloys
Melt the iron, then add the alloys
Charge the cut iron, put on the clay lids, fill the hole with coke and close the cover. Renew the fire as it burns through. Add the tungsten powder and ferro-alloys to the liquid iron and melt them in. Unknown: the melting time and temperature for this charge. The book says only that tool steel takes longer than ordinary steel. About 3½ tons of coke go to each ton of high-speed steel.
Alat yang dibutuhkan:
Tungku krusibel
Kokas metalurgi
Penjepit Kowi4
4
Pull out, skim and teem
Pull out, skim and teem
Lift each pot out with the pulling-out tongs (arms and legs covered with wet sacking), take off the lid and skim the slag with a mop, then pour the steel into ingot moulds. Unknown: the ingot size. A clay crucible lasts about 3 heats.
Alat yang dibutuhkan:
Penjepit Kowi
Cetakan batang logam
Sarung Tangan Tahan Panas5
5
Work the ingot into round bar
Work the ingot into round bar
Unknown: how the ingot is heated, hammered or rolled, and annealed into round bar. Carnegie and Gladwyn stop at the liquid steel, so this step is linked to an unknown head until a source gives it.
Alat yang dibutuhkan:
Jadwal tempa tak diketahuiBahan
5- 55 ponPlaceholder
- 26 ponPlaceholder
- 12 ponPlaceholder
- 9.5 ponPlaceholder
- 1 ponPlaceholder
Alat yang Diperlukan
9- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Cetak biru ini membuat
Blueprint terkait
Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip

Crucible Cast Steel by the Huntsman Process — Remelting Blister Steel into Flawless Ingots
oleh Tarkin
Pengerjaan Logam
48
0
0
0
0
0

Berbahaya
Ductile Tungsten Wire: Pressed, Sintered by Current, Swaged and Drawn Hot (Coolidge 1913)
oleh Forge
Pengerjaan Logam
2
0
0
0
0
0

High-Speed Steel, Charge 1: Crucible-Melted Tungsten-Chrome-Molybdenum Steel (Carnegie & Gladwyn 1918)
oleh Forge
Pengerjaan Logam
1
0
0
0
0
0
CC0 Domain Publik
Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.
Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.