Lactide: Lactic Acid Condensed and Cracked under Vacuum, Recrystallised
Charlie

Dibuat oleh

Charlie

19. Oktober 2026DE
11
0
0
0
0

Lactide: Lactic Acid Condensed and Cracked under Vacuum, Recrystallised

Lactide is the ring-shaped double molecule of lactic acid, the monomer from which PLA is made. Schneider's du Pont patent (US 2,703,316, 1955) drives the water out of lactic acid, condenses it under vacuum to a syrupy low polymer, then heats that to 200–250 °C at 8–10 mm so that lactide distils off. For a tough plastic it must be very pure: recrystallise it from ethyl acetate until it melts at 120 °C or higher (best 123–125 °C). The picture: our diagram.
Lanjutan
1–2 days

Instruksi

1

Drive off the water

Distil the lactic acid at atmospheric pressure at 120–130 °C until nearly all the water of dilution has gone.

Material untuk langkah ini:

Asam Laktat (teknis)Asam Laktat (teknis)1 buah

Alat yang dibutuhkan:

Labu alas bulatLabu alas bulat
Kumparan kondensorKumparan kondensor
Pelat PemanasPelat Pemanas
Penangas minyakPenangas minyak
Termometer LaboratoriumTermometer Laboratorium
2

Condense under vacuum

Continue distilling under 17–35 mm of mercury. Water of esterification comes off and the acid becomes a syrupy low polymer (polylactic acid).

Alat yang dibutuhkan:

Pompa vakumPompa vakum
Pengukur vakumPengukur vakum
Perangkap DinginPerangkap Dingin
Penangas minyakPenangas minyak
Termometer LaboratoriumTermometer Laboratorium
3

Crack to lactide

Lower the pressure to 8–10 mm and raise the temperature to 200–250 °C. Lactide distils at 130–140 °C (10–13 mm) and sets to a soft crystalline solid.

Alat yang dibutuhkan:

Pompa vakumPompa vakum
Pengukur vakumPengukur vakum
Kumparan kondensorKumparan kondensor
Penangas minyakPenangas minyak
Termometer LaboratoriumTermometer Laboratorium
Sarung Tangan Tahan PanasSarung Tangan Tahan Panas
4

Recrystallise from ethyl acetate

Recrystallise the crude lactide from ethyl acetate, filter and dry. Repeat: in the patent the melting point rose from 114–115 °C after the first crystallisation to 118, 123–124 and 124–125 °C after the fourth.

Alat yang dibutuhkan:

Etil AsetatEtil Asetat
Gelas Beker Kaca Tahan PanasGelas Beker Kaca Tahan Panas
Pelat PemanasPelat Pemanas
Corong Büchner (porselen)Corong Büchner (porselen)
Kertas SaringKertas Saring
Kacamata Pelindung Cipratan KimiaKacamata Pelindung Cipratan Kimia
5

Check the melting point

Put a few crystals in a capillary tube and warm slowly. Lactide melting at 120 °C or above is fit for making PLA; below 120 °C it gives a brittle polymer.

Alat yang dibutuhkan:

Tabung kapiler kacaTabung kapiler kaca
Termometer LaboratoriumTermometer Laboratorium
Penangas minyakPenangas minyak

Bahan

1

Alat yang Diperlukan

15

Cetak biru ini membuat

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...