Methyl Methacrylate Syrup: Partly Polymerised below 80 °C with Hydrogen Peroxide
Methyl methacrylate syrup is the monomer partly polymerised until it is thick: the stock that is poured between glass plates to cast acrylic sheet. ICI's Tattersall (US 2,071,907, 1937) heats the liquid monomer with a little catalyst, never above 80 °C, until it is syrupy, then cools it. His example used benzoyl peroxide and he names hydrogen peroxide as an alternative but gives no amount. Our choice: 14 g of 3 % hydrogen peroxide per kg of monomer, as many peroxide molecules as his 0.3 % benzoyl peroxide. Methyl methacrylate is flammable: no open flame.
The picture: our diagram.
Menengah
Half a day
Instruksi
1
1
Weigh monomer and peroxide
Weigh monomer and peroxide
Weigh liquid methyl methacrylate into a round-bottom flask and add 14 g of 3 % hydrogen peroxide per kg of monomer (our amount; the patent only says a relatively small amount).
Material untuk langkah ini:
Metil Metakrilat1 kg
Hidrogen peroksida (3 %)14 gAlat yang dibutuhkan:
Labu alas bulat
Neraca lengan
Kacamata Pelindung Cipratan Kimia
Sarung tangan karet
Lemari asam (bersaluran buang)2
2
Heat, never above 80 °C
Heat, never above 80 °C
Fit a reflux condenser and warm the flask in a water bath to near but not above 80 °C. Above 80 °C the finished sheet is not flawless; lower temperatures work but take longer.
Alat yang dibutuhkan:
Labu alas bulat
Kondensor Refluks
Penangas Air
Pelat Pemanas
Termometer Laboratorium
Lemari asam (bersaluran buang)3
3
Stop when it is syrupy
Stop when it is syrupy
Check the thickness now and then with a glass rod. Stop when the liquid has become a syrup. The patent took its example to a molecular weight of 3000, measured by viscosity, and gives no time.
Alat yang dibutuhkan:
Batang Pengaduk Kaca
Termometer Laboratorium4
4
Cool to room temperature
Cool to room temperature
Cool the syrup to about room temperature (30 °C in the example) in cold water. It is then ready to pour between glass plates and cast into sheet.
Alat yang dibutuhkan:
Bak pendingin air
Termometer Laboratorium
Sarung tangan karetBahan
2- 1 kgPlaceholder
- Placeholder
Alat yang Diperlukan
11- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Cetak biru ini membuat
Blueprint terkait
Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip
CC0 Domain Publik
Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.
Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.