Polypropylene Felt: a Spunbonded Web, Kinney 1967
Tex

Dibuat oleh

Tex

18. Oktober 2026FO
10
0
0
0
0

Polypropylene Felt: a Spunbonded Web, Kinney 1967

A polypropylene felt made without weaving or needling: hot filaments are spun, pulled down by an air jet, given an electric charge so they spread apart, and laid in loops on a moving table until they form an even sheet. Kinney's patent (Du Pont, US 3,338,992, 1967) gives every setting for polypropylene. The corona runs at 20 to 25 kV: keep clear of it while it is live. The picture: the patent's own Fig. 1 (the process) and Fig. 7 (the web).
Lanjutan
1 day

Instruksi

1

Melt and spin

Melt polypropylene of melt index 10 in a screw extruder, no hotter than 290 °C. Meter it at 12 g a minute through a 1/4 in. sand filter and a 20-hole spinneret (holes 0.015 in. across): pack block 275 °C, spinneret 260 °C.

Material untuk langkah ini:

Pelet polipropilenaPelet polipropilena500 g

Alat yang dibutuhkan:

Ekstruder plastikEkstruder plastik
Nosel pemintalNosel pemintal
PirometerPirometer
Neraca lenganNeraca lengan
Sarung Tangan KulitSarung Tangan Kulit
2

Quench

Cool the bundle of filaments in a 6 in. quench chimney blowing 40 cubic feet a minute of room air in from the side.

Alat yang dibutuhkan:

Kompresor udaraKompresor udara
3

Draw with the air jet

Lead the bundle 72 in. down into an air draw jet run at 25 psi: it pulls the filaments with about 3 g of tension and stretches them.

Alat yang dibutuhkan:

Jet penarik udaraJet penarik udara
Kompresor udaraKompresor udara
Pengukur TekananPengukur Tekanan
4

Charge the filaments

8 in. above the jet, let the filaments brush a 1 1/4 in. bar turning at 10 rpm, with a four-point corona 5/8 in. from it at minus 20 to 25 kV (100 to 150 µA). The charge pushes them apart. Keep clear while it is live.

Alat yang dibutuhkan:

Unit pengisian koronaUnit pengisian korona
5

Lay the web

Catch the filaments on a grounded 47 in. square table that moves 26 in. a minute one way and 570 in. a minute the other. Each layer weighs 0.5 oz per square yard; lay several for each sheet.

Alat yang dibutuhkan:

Meja penumpukMeja penumpuk
6

What you get

An even sheet of fine filaments, about 2.5 denier each, tenacity 2.0 g per denier, stretching 300 % before they break.

Alat yang dibutuhkan:

Neraca lenganNeraca lengan

Bahan

1

Alat yang Diperlukan

10

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.