Precipitated Silica: Hot Water Glass Carbonated, Then Acidified to pH 6.75 (Allen 1957)

Bubble carbon dioxide through hot dilute water glass and the silica comes down as an extremely fine white powder rather than a gel. Edward Allen of Columbia-Southern made it this way as a white reinforcing filler for rubber; this follows his Example XI, which gave a powder of 148 m² per gram. Source: E. M. Allen (Columbia-Southern), US 2,805,955 (1957), Example XI. The percentages are our arithmetic; the filter, mill and indicator are ours. Picture drawn by Youblob.
Menengah
2 days

Instruksi

1

Dilute the water glass

Take 12,850 g of sodium silicate solution holding 976 g Na2O and 3115 g SiO2 (7.6 % and 24.2 %, a silica to soda ratio of 3.19 by weight; our arithmetic). Dilute it with water to 48 litres in a stirred kettle with a heating coil and thermometer, and heat to 95 °C.

Material untuk langkah ini:

Kaca air (larutan natrium silikat)Kaca air (larutan natrium silikat)12850 g
AirAir1 as required

Alat yang dibutuhkan:

Reaktor bertekananReaktor bertekanan
PengadukPengaduk
TermometerTermometer
Neraca lenganNeraca lengan
2

Carbonate for an hour

Bubble in pure carbon dioxide fast enough to add the theoretical amount in about 30 minutes, and keep going at that rate for about 1 hour. The slurry ends at pH 9.85.

Alat yang dibutuhkan:

Gas karbon dioksidaGas karbon dioksida
Reaktor bertekananReaktor bertekanan
PengadukPengaduk
TermometerTermometer
Kertas indikator pHKertas indikator pH
3

Filter and wash

Filter the slurry and wash the cake twice with hot water.

Material untuk langkah ini:

AirAir1 as required

Alat yang dibutuhkan:

Corong Büchner (porselen)Corong Büchner (porselen)
Kertas SaringKertas Saring
4

Acidify to pH 6.75

Stir the cake back into water and bring it to pH 6.75 with 400 ml of 3.5 N hydrochloric acid.

Material untuk langkah ini:

AirAir1 as required

Alat yang dibutuhkan:

Asam kloridaAsam klorida
Wadah kacaWadah kaca
PengadukPengaduk
Kertas indikator pHKertas indikator pH
5

Wash out the chloride

Filter again and wash the cake with hot water until it is nearly free of chloride.

Material untuk langkah ini:

AirAir1 as required

Alat yang dibutuhkan:

Corong Büchner (porselen)Corong Büchner (porselen)
Kertas SaringKertas Saring
6

Dry at 105 °C and grind

Dry it at 105 °C in a fan oven and grind it to a fine powder. Allen's had a pH of 8.2, 0.61 % sodium and a surface area of 148 m² per gram.

Alat yang dibutuhkan:

Oven pengeringanOven pengeringan
Lumpang dan AluLumpang dan Alu
Toples Kaca BertutupToples Kaca Bertutup

Bahan

2

Alat yang Diperlukan

13

Cetak biru ini membuat

Blueprint terkait

Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...