PTFE Thread Seal Tape: Paste-Extruded, Calendered, Never Sintered
Emma

Dibuat oleh

Emma

26. Oktober 2026SE
4
0
0
0
0

PTFE Thread Seal Tape: Paste-Extruded, Calendered, Never Sintered

The white tape wound on pipe threads is PTFE that has never been melted. Fine PTFE powder is mixed with a lubricant, pressed into a slug, squeezed through a slit die by a ram, rolled thin between two rolls, and dried. Kept below the sintering heat (about 350 °C) it stays soft and conforms to the thread (process: US 5,415,939, 1995). The targets and tests are those of the Indian standard IS 14643 (from BS 4375): no fillers, at most 0.1 % lubricant left, usually 12 mm wide and 0.075 mm thick. The lubricant (naphtha) and the slitter are ours. The picture: Fig. 1a of the patent.
Lanjutan
1 day

Instruksi

1

Wet the powder

Mix fine (dispersion-made) virgin PTFE powder with a lubricant that can be driven off completely. Granular PTFE will not paste-extrude. No fillers. Ours: naphtha, as required.

Material untuk langkah ini:

Serbuk halus PTFESerbuk halus PTFE1 batch

Alat yang dibutuhkan:

NaftaNafta
2

Press a preform

Compact the wet powder into a cylindrical preform in a mould with a plunger.

Alat yang dibutuhkan:

Cetakan kompresiCetakan kompresi
Mesin pres hidrolikMesin pres hidrolik
3

Ram-extrude a flat tape

Put the preform in the extrusion press. The plunger pushes it out through a slit die as a thick flat tape.

Alat yang dibutuhkan:

Mesin tekan ekstrusi hidraulikMesin tekan ekstrusi hidraulik
4

Calender it thin

Pass the tape between two counter-rotating rolls to a thin tape, aiming at about 0.075 mm.

Alat yang dibutuhkan:

Mesin canai logamMesin canai logam
MikrometerMikrometer
5

Dry off the lubricant

Dry the tape until the lubricant is gone. Keep it well below the sintering heat (about 350 °C): sintered tape is stiff and will not seal.

Alat yang dibutuhkan:

Oven pengeringanOven pengeringan
6

Slit and spool

Slit it to width, usually 12 mm (±0.5 mm), and wind it on spools.

Alat yang dibutuhkan:

Mesin slitter-rewinderMesin slitter-rewinder
7

Check the tape

It must look white, with no visible specks or torn edges. Measure the thickness at five points along a sample; each must be within 10 % of their mean.

Alat yang dibutuhkan:

MikrometerMikrometer
8

Test the residual lubricant

Weigh about 15 g of tape. Extract it in a Soxhlet with petroleum spirit (40-60 °C) for at least 4 h, dry it at 100 °C, then heat it at 300 °C for 6 h, cool and weigh. The loss must be 0.1 % or less.

Alat yang dibutuhkan:

Ekstraktor SoxhletEkstraktor Soxhlet
Eter minyak bumiEter minyak bumi
Oven pengeringanOven pengeringan
Wadah lebur bajaWadah lebur baja
Ruang pengering (kecil)Ruang pengering (kecil)
Timbangan PresisiTimbangan Presisi
9

Wrap a thread

Wind tape round an R 1/2 taper pipe thread with 50 % overlap, two layers deep, just tight enough to take the thread form. It must hold the form, not break, and its end must stay put.

Alat yang dibutuhkan:

Sambungan pipa berulirSambungan pipa berulir

Bahan

1

Alat yang Diperlukan

14

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...