Reverberatory Furnace: the Air Furnace for Melting Cast Iron (Bolland, 1893)
Forge

Dibuat oleh

Forge

4. November 2026NO
13
0
0
0
0

Reverberatory Furnace: the Air Furnace for Melting Cast Iron (Bolland, 1893)

An air furnace melts iron apart from the fuel: coal burns on a grate at one end, and the flame is thrown down from a low arched roof onto the iron on the bed, then leaves by a tall chimney. The iron stays cleaner than in a cupola, so founders used it for guns, rolls, heavy scrap and lumps too big for the cupola. This furnace is 30 ft 6 in long and 7 ft wide outside, 5 ft wide inside, cased in bolted wrought-iron plates. Source: S. Bolland, The Iron Founder Supplement (1893), pp. 55-67. Unknown: brick sizes, plate thickness. Picture: Fig. 14 of the book.
Ahli
Unknown

Instruksi

1

Lay the foundation

Build the foundation solid of common material up to the firebrick, shaped so the firebrick bed slopes down from the chimney end to the reservoir. Keep the bricks from B to C 6 in below the finished bottom, to leave room for the sand bed.

Material untuk langkah ini:

BataBata1 foundation

Alat yang dibutuhkan:

Sendok semenSendok semen
Dimensi tidak diketahuiDimensi tidak diketahui
2

Build the fireplace, bridge and roof

Build the fireplace the full width of the furnace (5 ft inside, grate 5 ft long). Set the bridge wall at least 2 ft 3 in from the face of the grate bars. Build bridge, sides, roof and fireplace of the most refractory firebrick. Arch the roof the whole length, low, so it throws the flame down onto the bed; fill above the arches with common material. Leave the side charging hole (5 x 4 ft), the top hole (furnace width x 6 ft), the puddling hole over the reservoir, a sight hole and the tap hole.

Material untuk langkah ini:

Batu bata tanah apiBatu bata tanah api1 lining, bridge, roof
Adukan tanah liat tahan apiAdukan tanah liat tahan api1 setting
BataBata1 filling above the arch
Logam tidak diketahuiLogam tidak diketahui1 grate bars

Alat yang dibutuhkan:

Sendok semenSendok semen
3

Case it in plates and bolt it

Case the whole structure in wrought-iron plates, held at the corners with angle-irons. Run eight chief anchor bolts from side to side, clear of all working parts. Join everything with bolts, not rivets, so any plate can come off for repairs. Line the charging doors with firebrick.

Material untuk langkah ini:

Pelat besiPelat besi1 casing, doors
Tongkat besi tempaTongkat besi tempa8 anchor bolts
Logam tidak diketahuiLogam tidak diketahui1 angle-irons, door frames
Batu bata tanah apiBatu bata tanah api1 door linings

Alat yang dibutuhkan:

Dimensi tidak diketahuiDimensi tidak diketahui
4

Build the chimney

Build the chimney square, 30 to 40 ft high, with an inside course of firebrick (Fig. 14: 2 ft 6 in square inside). Make its area a little larger than the fireplace. Put a damper on top that can be worked from the bottom: it alone sets the draught. It can stand apart on a sole plate on four columns.

Material untuk langkah ini:

Batu bata tanah apiBatu bata tanah api1 inside course
BataBata1 chimney
Logam tidak diketahuiLogam tidak diketahui1 damper

Alat yang dibutuhkan:

Sendok semenSendok semen
5

Make the sand bottom

Make the bottom from B round the reservoir to C with 8 parts fire-sand to 1 of clay and 1 of ground coke. Fire it well for one to two hours before the first charge; it should last ten heats. Fill the tap hole with fire-sand and a little coal dust, which will not cake when hot.

Material untuk langkah ini:

PasirPasir8 parts
LempungLempung1 part
Kokas metalurgiKokas metalurgi1 part, ground

Alat yang dibutuhkan:

Batu bara bituminusBatu bara bituminus
6

Charge and melt

Fire with soft, non-caking bituminous coal and keep a full grate; clinker quickly and leave no holes for cold air. Charge all the iron at the start: first layer of pigs lengthwise and a little apart, next layers across, open so the flame passes. Set heavy pieces on firebricks so the flame plays all round them. Through the puddling hole, dip test pieces and skim the iron clean. To blend two grades, thrust green saplings into the melt. Close the damper before tapping. Look the furnace over after every heat.

Alat yang dibutuhkan:

Batu bara bituminusBatu bara bituminus
Batangan besi kasarBatangan besi kasar
Batang Pohon Muda Kayu KerasBatang Pohon Muda Kayu Keras
Serok berlubangSerok berlubang

Bahan

9

Alat yang Diperlukan

6

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...