Sandpaper from Sand, Hide Glue and Paper
Mary

Dibuat oleh

Mary

11. Oktober 2026FI
36
0
0
0
0

Sandpaper from Sand, Hide Glue and Paper

A coated abrasive is grit glued to a backing. The first recorded one, in 13th-century China, bonded crushed shells, seeds and sand to parchment with natural gum. Here clean quartz sand is crushed, sieved into grades and scattered on paper brushed with warm hide glue. Sieve mesh only roughly matches a shop grit number: real P grades are set by ISO 6344. Quartz grit on hide glue wears faster than garnet or aluminium oxide paper, and water softens the glue, so use it dry.
Pemula
1 hour, plus a day drying

Instruksi

1

Crush the sand

With a dust mask on, crush clean quartz sand in the mortar, a few spoonfuls at a time.

Material untuk langkah ini:

Pasir KuarsaPasir Kuarsa300 g

Alat yang dibutuhkan:

Lumpang dan AluLumpang dan Alu
Masker DebuMasker Debu
2

Sieve into grades

Sieve through the 60, 80 and 120 mesh sieves stacked coarse on top. Keep what each sieve holds in its own labelled jar: coarse, medium and fine.

Alat yang dibutuhkan:

Ayakan 60 meshAyakan 60 mesh
Ayakan mesh 80Ayakan mesh 80
Ayakan 120 MeshAyakan 120 Mesh
Toples Kaca BertutupToples Kaca Bertutup
Masker DebuMasker Debu
3

Warm the glue

Soak hide glue granules in water, then warm them in a double boiler to about 60 °C until runny. Do not let it boil.

Material untuk langkah ini:

Lem kulit hewanLem kulit hewan50 g
AirAir0.1 liter

Alat yang dibutuhkan:

Panci timPanci tim
Pelat PemanasPelat Pemanas
Termometer probe tinggal-pasangTermometer probe tinggal-pasang
4

Glue the paper

Brush a thin, even coat of glue over one face of a sheet of strong paper, edge to edge.

Material untuk langkah ini:

KertasKertas3 lembar

Alat yang dibutuhkan:

Kuas lemKuas lem
5

Scatter the grit

While the glue is wet, sprinkle one grade of grit thickly over it, press it in with a rolling pin over a clean sheet, and let it set for a minute.

Alat yang dibutuhkan:

Penggilas adonanPenggilas adonan
6

Shake off and dry

Tip the sheet on edge and tap off the loose grit back into its jar. Dry it flat for a day, then label the back with its grade.

Alat yang dibutuhkan:

Toples Kaca BertutupToples Kaca Bertutup
7

Test it

Sand a scrap of softwood ten strokes and look at the scratches. Cut sheets to size.

Alat yang dibutuhkan:

GuntingGunting
8

Troubleshooting

Home-made sandpaper troubleshooting.

Flow

Loading...

Bahan

4
  • Placeholder
  • Placeholder
  • 0.1 liter
    Placeholder
  • 3 lembar
    Placeholder

Alat yang Diperlukan

12

Blueprint terkait

Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.