Silver Solder of Silver and Red Copper With a Burnt Wine-Stone Flux (Theophilus, 12th Century)
Forge

Dibuat oleh

Forge

14. November 2026NO
9
0
0
0
0

Silver Solder of Silver and Red Copper With a Burnt Wine-Stone Flux (Theophilus, 12th Century)

How Theophilus soldered silver in the 12th century: an alloy of two parts pure silver and a third part red copper, rasped to filings, laid on a joint painted with a flux of burnt wine-stone (tartar) ground with water and salt, and flowed in the coals with a long gentle blast.
Menengah
About half a day

Instruksi

1

The alloy

Memuat notebook Jupyter…
2

Read De Diversis Artibus, Book III

"Weigh two parts of pure silver, and a third (part) of red copper, and mix and finely rasp into a clean vessel."
3

Make the solder

Weigh two parts of pure silver and a third part of red copper, melt them together, and rasp the alloy finely into a clean vessel; keep the filings in a quill.

Material untuk langkah ini:

Perak MurniPerak Murni1 buah
TembagaTembaga1 buah

Alat yang dibutuhkan:

Neraca lenganNeraca lengan
KowiKowi
Penjepit KowiPenjepit Kowi
Perapian pandai besiPerapian pandai besi
Ubub (Pengembus)Ubub (Pengembus)
Kikir kasarKikir kasar
Pena BuluPena Bulu
4

Make the flux

Take wine-stone from a vessel in which good wine has stood a long time, tie pieces in a cloth and put it in the fire until no more vapour comes from it. When cool, blow off the cloth ash and grind the burnt stone in a copper vessel with a round mallet, mixing in water and salt until it is as thick as lees.

Material untuk langkah ini:

Batu anggur mentah (kerak tong anggur)Batu anggur mentah (kerak tong anggur)1 buah
Kain KatunKain Katun1 buah
GaramGaram1 buah

Alat yang dibutuhkan:

Perapian pandai besiPerapian pandai besi
Ember 20 LiterEmber 20 Liter
Palu KayuPalu Kayu
5

Solder

With a thin piece of wood paint the flux round the joint inside and out, shake the filed solder over it with a small iron, and dry it. Paint more flux on, more thickly than before, put the work in the fire, cover it with coals and blow gently with a long breath until the solder has melted. Take it out, let it cool slightly and wash it. If the joint is not firm, do it again. Then file and scrape it smooth.

Alat yang dibutuhkan:

Perapian pandai besiPerapian pandai besi
Ubub (Pengembus)Ubub (Pengembus)
Penjepit KowiPenjepit Kowi
Kikir (Kikir Tangan)Kikir (Kikir Tangan)
6

Troubleshooting

Soldering troubleshooting.

Flow

Loading...
7

History and honest limits

From Theophilus, **De Diversis Artibus**, Book III, chapter XXXI, translated by Robert Hendrie (1847) (checked on the archive.org scan essayuponvarious00hend, pp. 241-243). "A third (part)" can be read two ways; both are shown. Melting the alloy before rasping, the tools and the diagram are ours.

Bahan

5

Alat yang Diperlukan

10

Cetak biru ini membuat

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...