Guitar Strings: Bronze Wound on Steel, Then Heat-Soaked (Stone and Falcone 1977)
A wound string is a steel core with another wire wrapped round it. Stone and Falcone believed the wrap keeps stresses from the winding and slowly unwinds as the string is played, so the tone goes dead. Their fix: after winding, heat-soak the string, at least 2 hours at 270 °F or 30 minutes at 480 °F for a bronze wrap, then let it cool.
Source: W. N. Stone and A. S. Falcone (National Musical String Co.), US 4,063,674 (1977). Unknown: the winding itself (the patent calls it conventional), where phosphor bronze wire comes from, and the gauges. These are linked to unknown heads. The plain strings of the set are steel music wire; that, the oven and the nitrogen are ours. Picture drawn by Youblob.
Lanjutan
1 day
Instruksi
1
1
Cut the core and plain strings
Cut the core and plain strings
Cut steel music wire for the cores of the wound strings and for the plain strings of the set. Unknown: the gauges and lengths, and the ball ends.
Material untuk langkah ini:
Kawat Musik Baja 0,032"1 as requiredAlat yang dibutuhkan:
Tang potong
Dimensi tidak diketahui2
2
Wind the bronze wrap at room temperature
Wind the bronze wrap at room temperature
Wrap phosphor bronze wire helically round each core at room temperature. The patent prefers a wrap that expands more with heat than the core. Unknown: how; the patent says only 'in a conventional manner'.
Material untuk langkah ini:
Kawat perunggu fosfor1 as requiredAlat yang dibutuhkan:
Metode lilitan tak diketahui
Dimensi tidak diketahui
Kacamata pengaman3
3
Heat-soak the wound strings
Heat-soak the wound strings
Heat the wound strings for a bronze wrap at 270-480 °F (132-249 °C): at least 2 hours at 270 °F or at least 30 minutes at 480 °F, shorter the hotter. If the wire tarnishes in hot air, do it without air, in nitrogen or carbon dioxide. The wrap's turns settle into more even spacing.
Alat yang dibutuhkan:
Oven
Termometer Laboratorium
Tabung Gas Nitrogen4
4
Cool and set up the set
Cool and set up the set
Let the strings cool back to room temperature. Make up the set with the plain steel strings.
Alat yang dibutuhkan:
Tang potongBahan
2- 1 as requiredPlaceholder
- 1 as requiredPlaceholder
Alat yang Diperlukan
7- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Cetak biru ini membuat
Blueprint terkait
Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip
CC0 Domain Publik
Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.
Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.