A varistor made the other way round: a disc of pure zinc oxide, sintered, with bismuth oxide fired into its faces from a paste instead of mixed in. Sintered at 1350 °C and fired with the paste at 800 °C, the disc measured a C-value of 90 at 1 mA and a nonlinearity exponent n of 7.3. Masuyama found that firing on the bismuth oxide paste raises n a great deal over mixing it in. Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 4. Unknown: how the aluminium is sprayed on, what the silver paint is, and how strong the epoxy solution of the paste is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
Lanjutan
2 days

Instruksi

1

Press pure zinc oxide at 340 kg/cm²

Press zinc oxide powder at 340 kg/cm². Example 4 gives no disc size; ours: discs 13 mm across and 2.5 mm thick in the mould of Example 1.

Material untuk langkah ini:

Serbuk Seng OksidaSerbuk Seng Oksida1 as required

Alat yang dibutuhkan:

Neraca lenganNeraca lengan
Mesin pres hidrolikMesin pres hidrolik
Cetakan press cakramCetakan press cakram
Jangka Sorong VernierJangka Sorong Vernier
2

Sinter 1 hour at 1350 °C and cool

Heat the pressed disc for 1 hour at 1350 °C, then let it cool to room temperature.

Alat yang dibutuhkan:

Tungku MuffleTungku Muffle
3

Lap both faces

Lap both faces with silicon carbide abrasive. Example 4 gives no thickness.

Alat yang dibutuhkan:

Butiran silikon karbidaButiran silikon karbida
Jangka Sorong VernierJangka Sorong Vernier
4

Coat with bismuth oxide paste and fire at 800 °C

Coat both lapped faces with a paste of 50 % by weight bismuth oxide in a solution of epoxy resin in butyl alcohol, and fire it in air at 800 °C for 30 minutes. The bismuth oxide diffuses into the zinc oxide. Not given: how much paste, or the strength of the epoxy solution.

Material untuk langkah ini:

Bismut oksidaBismut oksida1 as required

Alat yang dibutuhkan:

Resin epoksiResin epoksi
n-Butanoln-Butanol
Tungku MuffleTungku Muffle
5

Spray aluminium electrodes and attach leads

Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint, as in Example 1. Unknown: the spraying method and the paint.

Material untuk langkah ini:

Batangan aluminiumBatangan aluminium1 as required
Cat perak penghantar listrikCat perak penghantar listrik1 as required
Kawat TembagaKawat Tembaga2 buah

Alat yang dibutuhkan:

Metode semprot logam yang tidak diketahuiMetode semprot logam yang tidak diketahui
Jangka Sorong VernierJangka Sorong Vernier

Bahan

5

Alat yang Diperlukan

9

Blueprint terkait

Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...