Metal Oxide Varistor: Zinc Oxide with Bismuth and Nickel Oxides, 1350 °C (Masuyama 1972)
Masuyama, Matsuoka and Nishi found that adding a second oxide to zinc oxide and bismuth oxide changes the varistor a great deal. This is their Example 2 with nickel oxide: 99.0 % zinc oxide, 0.5 % bismuth oxide and 0.5 % nickel oxide by moles, sintered at 1350 °C. The disc measured a C-value of 49 at 1 mA and a nonlinearity exponent n of 8.8.
Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 2. Unknown: how the aluminium is sprayed on and what the silver paint is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
Lanjutan
1 day
Instruksi
1
1
Weigh 99.0 : 0.5 : 0.5 and wet-mill 5 hours
Weigh 99.0 : 0.5 : 0.5 and wet-mill 5 hours
Mix zinc oxide, bismuth oxide and nickel oxide 99.0 : 0.5 : 0.5 by moles. Ours, for 10 g: 9.675 g zinc oxide, 0.28 g bismuth oxide, 0.045 g nickel oxide (our arithmetic). Mill wet for 5 hours, then dry. Unknown: the milling liquid.
Material untuk langkah ini:
Serbuk Seng Oksida9.675 g
Bismut oksida0.28 g
Nikel Monoksida0.045 gAlat yang dibutuhkan:
Neraca lengan
Ball Mill Besi
Oven pengeringan2
2
Press discs 13 mm by 2.5 mm
Press discs 13 mm by 2.5 mm
Press the powder in a mould into discs 13 mm across and 2.5 mm thick at 340 kg/cm², as in Example 1.
Alat yang dibutuhkan:
Mesin pres hidrolik
Cetakan press cakram
Jangka Sorong Vernier3
3
Sinter 1 hour at 1350 °C and furnace-cool
Sinter 1 hour at 1350 °C and furnace-cool
Sinter the discs in air at 1350 °C for 1 hour, then let them cool in the furnace to room temperature (about 15-30 °C).
Alat yang dibutuhkan:
Tungku Muffle4
4
Lap to 10 mm by 1.5 mm
Lap to 10 mm by 1.5 mm
Lap both faces with 600-mesh silicon carbide. The finished disc is 10 mm across and 1.5 mm thick.
Alat yang dibutuhkan:
Jangka Sorong Vernier5
5
Spray aluminium electrodes and attach leads
Spray aluminium electrodes and attach leads
Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint. Unknown: the spraying method and the paint.
Material untuk langkah ini:
Batangan aluminium1 as required
Cat perak penghantar listrik1 as required
Kawat Tembaga2 buahAlat yang dibutuhkan:
Metode semprot logam yang tidak diketahui
Jangka Sorong VernierBahan
6- 9.675 gPlaceholder
- 0.28 gPlaceholder
- 0.045 gPlaceholder
- 1 as requiredPlaceholder
- 1 as requiredPlaceholder
- 2 buahPlaceholder
Alat yang Diperlukan
9- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Cetak biru ini membuat
Blueprint terkait
Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip
CC0 Domain Publik
Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.
Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.