Barium Ferrite Disc Magnet: Fired in Carbon Dioxide, Pressed at 12 t/cm² (Went, Philips 1956, Ex. 33)
A barium ferrite made with more iron oxide, 0.4 mol barium carbonate to 3.6 mol, fired an hour at 1300 °C in carbon dioxide. Little oxygen gives the hexagonal crystal BaFe18O27, with some iron in the lower state. It is milled again, bound with nitrocellulose or polyvinyl alcohol, and pressed hard at 12 tonnes per cm². Went's rod held 1,260 gauss with a coercive force of 700 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 33. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
उन्नत
2 days
निर्देश
1
1
Weigh barium carbonate and iron oxide
Weigh barium carbonate and iron oxide
Weigh 79.4 g barium carbonate (0.4 mol) and 580.9 g ferric oxide (3.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
इस चरण के लिए सामग्री:
बेरियम कार्बोनेट (विदराइट)79.4 ग्रा
फेरिक ऑक्साइड580.9 ग्राआवश्यक उपकरण:
तराजू
रबर के दस्ताने
P100 श्वासयंत्र2
2
Mill 15.5 hours, press a pastille, fire in CO2
Mill 15.5 hours, press a pastille, fire in CO2
Grind with alcohol in a ball mill for 15.5 hours, dry, and press into a pastille. Heat it at 1300 °C in carbon dioxide for 1 hour (ours: a tube furnace fed from a CO2 cylinder).
आवश्यक उपकरण:
लोहे की बॉल मिल
एथेनॉल - प्रयोगशाला श्रेणी, 95 %
सुखाने की भट्ठी
हाइड्रोलिक प्रेस
डिस्क दबाने की डाई
ट्यूब फ़र्नेस
कार्बन डाइऑक्साइड गैस
दाब वाली गैस का सिलिंडर
ताप-रोधी दस्ताने3
3
Pulverise, mill 14 hours, bind
Pulverise, mill 14 hours, bind
Crush the cooled pastille and grind it with alcohol for 14 hours. Press the powder into a pastille again with a ceramic binder (ours: polyvinyl alcohol, one of the two named), then crush it to grains.
इस चरण के लिए सामग्री:
पॉलीविनाइल अल्कोहल पाउडर1 as requiredआवश्यक उपकरण:
लोहे की बॉल मिल
एथेनॉल - प्रयोगशाला श्रेणी, 95 %
हाइड्रोलिक प्रेस
डिस्क दबाने की डाई4
4
Press at 12 tonnes per cm²
Press at 12 tonnes per cm²
Press the grains at 12 tonnes per cm² (ours: discs instead of rods). The patent describes no further firing.
आवश्यक उपकरण:
हाइड्रोलिक प्रेस
डिस्क दबाने की डाई5
5
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
आवश्यक उपकरण:
विद्युत-चुंबक
दिक्सूचकसामग्री
3- 79.4 ग्राप्लेसहोल्डर
- 580.9 ग्राप्लेसहोल्डर
- 1 as requiredप्लेसहोल्डर
आवश्यक उपकरण
14- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
यह ब्लूप्रिंट बनाता है
संबंधित ब्लूप्रिंट
ये ब्लूप्रिंट ज्ञान साझा करते हैं — तकनीक, सामग्री या सिद्धांत
CC0 पब्लिक डोमेन
यह ब्लूप्रिंट CC0 के तहत जारी किया गया है। आप बिना अनुमति माँगे इस कार्य को किसी भी उद्देश्य के लिए कॉपी, संशोधित, वितरित और उपयोग करने के लिए स्वतंत्र हैं।
उनके ब्लूप्रिंट के माध्यम से उत्पाद खरीदकर मेकर का समर्थन करें जहाँ वे मेकर कमीशन कमाते हैं जो विक्रेताओं द्वारा निर्धारित होता है, या इस ब्लूप्रिंट का नया संस्करण बनाएँ और राजस्व साझा करने के लिए इसे अपने ब्लूप्रिंट में कनेक्शन के रूप में शामिल करें।