Blister Copper: Matte Blown in a Quartz-Lined Converter (Parrot Works, Butte, Peters 1905)
खतरनाक
Charlie

द्वारा बनाया गया

Charlie

1. नवंबर 2026DE
5
0
0
0
0

Blister Copper: Matte Blown in a Quartz-Lined Converter (Parrot Works, Butte, Peters 1905)

Air blown through molten matte burns its iron and sulphur: first the iron goes into a slag with the silica of the converter's quartz lining, then the sulphur leaves the copper sulphide and metallic copper remains. Result: blister copper of up to over 99 %, poured in pigs of 215 to 275 lb; a 55 % matte took about 39 minutes to slag and 44 minutes to make copper. Source: Edward D. Peters, Modern Copper Smelting (1905), ch. XVII, Parrot practice; picture: his Plate XVI, converters. Not given: the remelting cupola charge. The blow gives off sulphur dioxide, a poisonous gas.
उन्नत
2 hours

खतरनाक सामग्री

इस ब्लूप्रिंट में खतरनाक प्रक्रियाएँ हैं। चरण-दर-चरण निर्देश देखने के लिए लॉग इन करें और अपनी खाता सेटिंग में खतरनाक सामग्री सक्षम करें।

साइन इन

यह ब्लूप्रिंट बनाता है

संबंधित ब्लूप्रिंट

ये ब्लूप्रिंट ज्ञान साझा करते हैं — तकनीक, सामग्री या सिद्धांत

CC0 पब्लिक डोमेन

यह ब्लूप्रिंट CC0 के तहत जारी किया गया है। आप बिना अनुमति माँगे इस कार्य को किसी भी उद्देश्य के लिए कॉपी, संशोधित, वितरित और उपयोग करने के लिए स्वतंत्र हैं।

उनके ब्लूप्रिंट के माध्यम से उत्पाद खरीदकर मेकर का समर्थन करें जहाँ वे मेकर कमीशन कमाते हैं जो विक्रेताओं द्वारा निर्धारित होता है, या इस ब्लूप्रिंट का नया संस्करण बनाएँ और राजस्व साझा करने के लिए इसे अपने ब्लूप्रिंट में कनेक्शन के रूप में शामिल करें।

चर्चा

(0)

लॉग इन करें चर्चा में शामिल होने के लिए

टिप्पणियाँ लोड हो रही हैं...