Copper Concentrate: Sulphide Ore Stamped, Jigged and Tabled at the Anaconda Mill (Richards, Ore Dressing 1903)
Copper sulphide ore is too lean to smelt as mined. At the Anaconda mill it was screened, crushed under steam stamps, sorted by settling speed in rising water, and run over jigs and slime tables, where the heavy copper minerals sink and the light quartz and feldspar wash away.
Result: concentrates of 12 to 20 % copper; 100 tons of ore gave 50 to 75 tons. The mill handled 2,500 to 2,700 tons a day.
Source: Robert H. Richards, Ore Dressing vol. II (1903), pp. 984-986, Mill No. 42, Anaconda Copper Mining Company. Not given: the copper in the ore, water per ton. Picture drawn by Youblob.
उन्नत
1 day
निर्देश
1
1
Sort the ore
Sort the ore
In the mine, pick the ore by hand into rich ore (straight to the smelter), hard concentrating ore and soft concentrating ore. The ore holds chalcocite, chalcopyrite, pyrite, enargite and blende in quartz and decomposed feldspar; the aim is to save the copper and silver without the zinc.
इस चरण के लिए सामग्री:
सल्फाइड ताँबा अयस्क100 tons2
2
Screen and pick
Screen and pick
Pass each kind over vibrating grizzlies with 1 in spaces; hand-pick the oversize for rich ore. Screen the undersize in trommels: 6.35 mm round holes for hard ore; 12.7 mm then 6.35 mm for soft ore.
आवश्यक उपकरण:
वर्गीकरण की छलनी
ट्रोमेल3
3
Crush under steam stamps
Crush under steam stamps
Crush the coarse hard ore under steam stamps with screens of 4.76 x 9.52 mm slots, the soft ore under stamps with 12.7 mm round holes. Richards notes that steam stamps were later given up for these ores.
आवश्यक उपकरण:
स्टैम्प मिल
जल4
4
Classify and jig
Classify and jig
Jig the coarse soft ore on 1-sieve Harz jigs. Send all fine ore to hydraulic classifiers with three spigots; each spigot feeds its own row of 2-sieve Collom jigs. The heavy concentrate is drawn from the jigs; middlings are crushed again.
आवश्यक उपकरण:
अयस्क जिग
जलीय वर्गीकारक
जल5
5
Table the slimes and collect
Table the slimes and collect
Run the classifier overflow over convex revolving slime tables. Gather all concentrates and settlings for the smelter: 12 to 20 % copper, 50 to 75 tons from 100 tons of ore. Tailings keep 1 1/4 to 2 % copper.
आवश्यक उपकरण:
घूमने वाली स्लाइम टेबल
तलछट टैंकसामग्री
1- 100 tonsप्लेसहोल्डर
यह ब्लूप्रिंट बनाता है
CC0 पब्लिक डोमेन
यह ब्लूप्रिंट CC0 के तहत जारी किया गया है। आप बिना अनुमति माँगे इस कार्य को किसी भी उद्देश्य के लिए कॉपी, संशोधित, वितरित और उपयोग करने के लिए स्वतंत्र हैं।
उनके ब्लूप्रिंट के माध्यम से उत्पाद खरीदकर मेकर का समर्थन करें जहाँ वे मेकर कमीशन कमाते हैं जो विक्रेताओं द्वारा निर्धारित होता है, या इस ब्लूप्रिंट का नया संस्करण बनाएँ और राजस्व साझा करने के लिए इसे अपने ब्लूप्रिंट में कनेक्शन के रूप में शामिल करें।