Ebonite (Hard Rubber)
Vulcanised rubber is rubber with a few sulphur bridges between its chains. Keep adding sulphur and the bridges multiply until the chains cannot move at all: the soft, stretchy material turns into a hard black solid you can turn on a lathe, polish like ebony and use as an electrical insulator.
**US 8,075**, "Improvement in the Manufacture of India Rubber", Nelson Goodyear (brother of Charles), granted 6. May 1851, claims "the combining of india-rubber and sulphur… for making a hard and inflexible substance hitherto unknown": about equal parts by weight, heated to 260–275 °F for three to six hours. It was one of the first rigid materials made by chemically changing a natural polymer, over half a century before Bakelite.
**You turn a part from commercial ebonite rod and measure what the sulphur did** — its density, and its charge when rubbed. Curing ebonite needs a heated press and releases hydrogen sulphide, so the blueprint starts from finished rod; the notebook does the chemistry.
मध्यवर्ती
3 hours
निर्देश
1
1
Cut the blank
Cut the blank
Clamp 20 mm ebonite rod in the vise between soft jaws. Saw off 60 mm. Ebonite chips like hard wood; saw slowly to avoid cracking the end.
इस चरण के लिए सामग्री:
एबोनाइट छड़1 टुकड़ाआवश्यक उपकरण:
हैक्सॉ
बेंच शिकंजा
इस्पात का पैमाना
पारदर्शी सुरक्षा चश्मा2
2
Chuck and face
Chuck and face
Grip 20 mm of the blank in the lathe's 3-jaw chuck. Face the end square with a sharp HSS tool at about 800 rpm, light cuts.
आवश्यक उपकरण:
धातु खराद
खराद औज़ार सेट (HSS)
पारदर्शी सुरक्षा चश्मा
धूल मास्क3
3
Turn to 16 mm
Turn to 16 mm
Turn 40 mm of length down to 16.0 mm. Check with the caliper every pass. The chips smell of sulphur - that is the bonded sulphur you measure later.
आवश्यक उपकरण:
धातु खराद
खराद औज़ार सेट (HSS)
डिजिटल वर्नियर कैलिपर, 6 इंच4
4
Drill the bore
Drill the bore
Spot the centre with a centre drill, then drill 3 mm through 35 mm from the tailstock. Clear chips every 5 mm - ebonite heats and gums if packed.
आवश्यक उपकरण:
सेंटर ड्रिल सेट
डिब्बे में बरमों का सेट
धातु खराद5
5
Taper the grip
Taper the grip
Set the compound to a shallow angle and taper 25 mm from 16 mm down to 10 mm. This is a fountain-pen grip section, the job ebonite still does today.
आवश्यक उपकरण:
धातु खराद
खराद औज़ार सेट (HSS)
डिजिटल वर्नियर कैलिपर, 6 इंच6
6
Sand and polish
Sand and polish
At low speed, sand 400 then 800 grit, then run the Micro-Mesh grits in order. Finish with polishing compound on a cloth. Ebonite takes a deep gloss without lacquer.
इस चरण के लिए सामग्री:
रेगमाल2 शीट
चमकाने का लेप5 ग्राआवश्यक उपकरण:
सूक्ष्म जाली रेगमाल किट (9 दाने)
धातु खराद
धूल मास्क7
7
Part off
Part off
Part off at 45 mm with the parting tool. Chamfer the cut end by hand with 800 grit.
आवश्यक उपकरण:
खराद औज़ार सेट (HSS)
धातु खराद8
8
Measure the density
Measure the density
Weigh the part. Drop it into 50 ml of water in the graduated cylinder and read the rise. Do the same with a bundle of rubber bands. Enter both in the notebook.
इस चरण के लिए सामग्री:
रबर बैंड1 पैकआवश्यक उपकरण:
परिशुद्ध डिजिटल तराज़ू
अंशांकित सिलिंडर9
9
Rub it and pick up paper
Rub it and pick up paper
Tear tissue into 5 mm scraps. Rub the ebonite 10 strokes on wool felt and hold it 2 cm above the scraps. Repeat with an acrylic offcut. Count scraps lifted by each.
इस चरण के लिए सामग्री:
अम्लरहित महीन काग़ज़1 शीट
एक्रिलिक शीट1 टुकड़ाआवश्यक उपकरण:
ऊनी नमदा10
10
The sulphur arithmetic
The sulphur arithmetic
Jupyter नोटबुक लोड हो रही है…
11
11
History & Context
History & Context
**What the patent specifies:** rubber and sulphur in about equal parts (or 2 : 1 with magnesia or lime), 260–275 °F, three to six hours. **Modern build (derived):** commercial ebonite rod, typically 25–32 % sulphur - the notebook shows why more than about 32 % cannot bond.
Ebonite was named for ebony, which it replaced in combs, pipe stems and instrument parts. It became a standard insulator of the electrical age and is still preferred for fountain-pen feeds because ink wets it. Its limits: it softens with heat, fades to brown and smells of sulphur in sunlight as the surface oxidises, and is brittle under impact.
सामग्री
6- 1 टुकड़ाप्लेसहोल्डर
- 2 शीटप्लेसहोल्डर
- 5 ग्राप्लेसहोल्डर
- 1 पैकप्लेसहोल्डर
- 1 शीटप्लेसहोल्डर
- 1 टुकड़ाप्लेसहोल्डर
आवश्यक उपकरण
14- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- सेंटर ड्रिल सेट10% कमीशनप्लेसहोल्डर
- प्लेसहोल्डर
- सूक्ष्म जाली रेगमाल किट (9 दाने)10% कमीशनप्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
संबंधित ब्लूप्रिंट
ये ब्लूप्रिंट ज्ञान साझा करते हैं — तकनीक, सामग्री या सिद्धांत
CC0 पब्लिक डोमेन
यह ब्लूप्रिंट CC0 के तहत जारी किया गया है। आप बिना अनुमति माँगे इस कार्य को किसी भी उद्देश्य के लिए कॉपी, संशोधित, वितरित और उपयोग करने के लिए स्वतंत्र हैं।
उनके ब्लूप्रिंट के माध्यम से उत्पाद खरीदकर मेकर का समर्थन करें जहाँ वे मेकर कमीशन कमाते हैं जो विक्रेताओं द्वारा निर्धारित होता है, या इस ब्लूप्रिंट का नया संस्करण बनाएँ और राजस्व साझा करने के लिए इसे अपने ब्लूप्रिंट में कनेक्शन के रूप में शामिल करें।