A soft ferrite ring core for coils and transformers: copper, zinc and iron oxides with a little brownstone, presintered once at 900 °C, pressed into a ring and sintered at 1100 °C in oxygen. Snoek's ring had an initial permeability of 148.
Source: J. L. Snoek, US 2,452,530 (Philips, 1948), Example I and its table. The violet iron oxide has its own blueprint (precipitated hematite calcined at 1000-1100 °C, after Nurdini et al. 2022); Snoek does not say how his was made. Picture: the patent's Fig. 4, the ring core.
उन्नत
2 days
निर्देश
1
1
Weigh 20 : 30 : 50 mol % and 1 % brownstone
Weigh 20 : 30 : 50 mol % and 1 % brownstone
Mix 20 mol % pure copper oxide, 30 mol % pure zinc oxide and 50 mol % pure violet iron oxide, and add 1 % by weight of brownstone (manganese dioxide). Ours, by weight: 13.24 g copper oxide, 20.32 g zinc oxide and 66.44 g iron oxide per 100 g, plus 1 g brownstone. Snoek does not say what makes it 'violet'; violet iron oxide has its own blueprint.
इस चरण के लिए सामग्री:
कॉपर ऑक्साइड13.24 ग्रा
ज़िंक ऑक्साइड चूर्ण20.32 ग्रा
बैंगनी आयरन ऑक्साइड66.44 ग्रा
मैंगनीज़ डाइऑक्साइड (पाइरोलुसाइट)1 ग्राआवश्यक उपकरण:
तराजू
धूल मास्क2
2
Grind half an hour in an iron ball mill
Grind half an hour in an iron ball mill
Grind the mixture for half an hour in a mill with iron balls.
आवश्यक उपकरण:
लोहे की बॉल मिल
धूल मास्क3
3
Presinter at 900 °C for 2 hours in oxygen
Presinter at 900 °C for 2 hours in oxygen
Heat the ground powder to 900 °C for 2 hours in oxygen and let it cool.
आवश्यक उपकरण:
ट्यूब फ़र्नेस
ऑक्सीजन
दाब वाली गैस का सिलिंडर
पाइरोमीटर
ढक्कन सहित मूषा (चीनी-मिट्टी)
ताप-रोधी दस्ताने4
4
Grind 2 hours with iron balls
Grind 2 hours with iron balls
Grind it for 2 hours in a disintegrator with iron balls.
आवश्यक उपकरण:
लोहे की बॉल मिल
धूल मास्क5
5
Press a ring at 4 tons per cm²
Press a ring at 4 tons per cm²
Press the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm cross-section.
आवश्यक उपकरण:
हाइड्रोलिक प्रेस
वलय दाबन डाई
धूल मास्क6
6
Sinter at 1100 °C in oxygen, cool 5–10 °C a minute
Sinter at 1100 °C in oxygen, cool 5–10 °C a minute
Sinter the ring at 1100 °C in a current of oxygen. Example I heats for 1 hour and cools in the oxygen at 5 to 10 °C per minute. Snoek's ring had an initial permeability of 148, measured at room temperature at 2 kHz.
आवश्यक उपकरण:
ट्यूब फ़र्नेस
ऑक्सीजन
दाब वाली गैस का सिलिंडर
पाइरोमीटर
क्रूसिबल चिमटा
ताप-रोधी दस्तानेसामग्री
4- 13.24 ग्राप्लेसहोल्डर
- 20.32 ग्राप्लेसहोल्डर
- 66.44 ग्राप्लेसहोल्डर
- प्लेसहोल्डर
आवश्यक उपकरण
12- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
यह ब्लूप्रिंट बनाता है
संबंधित ब्लूप्रिंट
ये ब्लूप्रिंट ज्ञान साझा करते हैं — तकनीक, सामग्री या सिद्धांत
CC0 पब्लिक डोमेन
यह ब्लूप्रिंट CC0 के तहत जारी किया गया है। आप बिना अनुमति माँगे इस कार्य को किसी भी उद्देश्य के लिए कॉपी, संशोधित, वितरित और उपयोग करने के लिए स्वतंत्र हैं।
उनके ब्लूप्रिंट के माध्यम से उत्पाद खरीदकर मेकर का समर्थन करें जहाँ वे मेकर कमीशन कमाते हैं जो विक्रेताओं द्वारा निर्धारित होता है, या इस ब्लूप्रिंट का नया संस्करण बनाएँ और राजस्व साझा करने के लिए इसे अपने ब्लूप्रिंट में कनेक्शन के रूप में शामिल करें।