Potash Alum from Alum Shale
Alum shale is a mix of iron pyrites, clay (aluminium silicate) and bituminous matter. Left to weather in the air, the pyrites oxidise and form sulphuric acid, which attacks the clay and turns it into aluminium sulphate. Water draws this out as a solution, which is settled, boiled down until iron sulphate crystallises out on cooling, then boiled down further to a specific gravity of 1.40. Stirred with the right amount of potassium sulphate, it throws down potash alum as a fine powder, alum meal. Alum crystallises in regular octahedra and is very soluble in water. Shale was also roasted to speed this up, which gives off sulphur dioxide; that route is not used here.
उन्नत
Weeks (weathering) plus days
निर्देश
1
1
Weather the shale
Weather the shale
Spread the broken shale in the open and let it weather, so the pyrites oxidise and the acid formed turns the clay into aluminium sulphate.
इस चरण के लिए सामग्री:
फिटकरी शेल1 as required2
2
Extract
Extract
Wash the weathered mass with water, step by step, until the solution reaches a specific gravity of 1.16.
इस चरण के लिए सामग्री:
जल1 as requiredआवश्यक उपकरण:
घनत्वमापी3
3
Settle
Settle
Let the solution stand so calcium sulphate and basic iron sulphate settle out, then draw it off.
आवश्यक उपकरण:
तलछट टैंक4
4
Remove the iron
Remove the iron
Boil it down until iron (ferrous) sulphate crystallises on cooling; draw off the liquor and boil it down to a specific gravity of 1.40.
आवश्यक उपकरण:
वाष्पन कड़ाह
घनत्वमापी5
5
Precipitate the alum
Precipitate the alum
Let it stand, decant it from any sediment, add the calculated amount of potassium sulphate and stir well: the alum falls as a fine powder, alum meal. (With much iron present, potassium chloride is used instead.)
इस चरण के लिए सामग्री:
पोटैशियम सल्फ़ेट1 as requiredआवश्यक उपकरण:
तलछट टैंकसामग्री
3- 1 as requiredप्लेसहोल्डर
- 1 as requiredप्लेसहोल्डर
- 1 as requiredप्लेसहोल्डर
यह ब्लूप्रिंट बनाता है
संबंधित ब्लूप्रिंट
ये ब्लूप्रिंट ज्ञान साझा करते हैं — तकनीक, सामग्री या सिद्धांत
CC0 पब्लिक डोमेन
यह ब्लूप्रिंट CC0 के तहत जारी किया गया है। आप बिना अनुमति माँगे इस कार्य को किसी भी उद्देश्य के लिए कॉपी, संशोधित, वितरित और उपयोग करने के लिए स्वतंत्र हैं।
उनके ब्लूप्रिंट के माध्यम से उत्पाद खरीदकर मेकर का समर्थन करें जहाँ वे मेकर कमीशन कमाते हैं जो विक्रेताओं द्वारा निर्धारित होता है, या इस ब्लूप्रिंट का नया संस्करण बनाएँ और राजस्व साझा करने के लिए इसे अपने ब्लूप्रिंट में कनेक्शन के रूप में शामिल करें।