Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1200 °C (Went, Philips 1956, Ex. 34)
A strontium ferrite magnet made exactly like Went's barium ferrite of Example 34, with strontium carbonate in place of barium carbonate: 29.5 g of it to 191.7 g iron oxide, milled, fired, milled again, pressed and sintered for 4 hours. This iteration sinters at 1200 °C, where his rod held 1,340 gauss with a coercive force of 3,900 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 34. They pressed rods; the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
उन्नत
2 days
निर्देश
1
1
Weigh strontium carbonate and iron oxide
Weigh strontium carbonate and iron oxide
Weigh 29.5 g of strontium carbonate and 191.7 g of ferric oxide, Fe2O3. The patent makes this second mixture "in exactly the same manner" as the barium one.
इस चरण के लिए सामग्री:
स्ट्रॉन्शियम कार्बोनेट29.5 ग्रा
फेरिक ऑक्साइड191.7 ग्राआवश्यक उपकरण:
तराजू
रबर के दस्ताने
P100 श्वासयंत्र2
2
Mill with ethanol for 4 hours
Mill with ethanol for 4 hours
Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.
आवश्यक उपकरण:
लोहे की बॉल मिल
एथेनॉल - प्रयोगशाला श्रेणी, 95 %
सुखाने की भट्ठी3
3
Presinter at 1000 °C for 4 hours
Presinter at 1000 °C for 4 hours
Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.
आवश्यक उपकरण:
मफल भट्ठी
ढक्कन सहित मूषा (चीनी-मिट्टी)
क्रूसिबल चिमटा
ताप-रोधी दस्ताने4
4
Mill again for 4 hours
Mill again for 4 hours
Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.
आवश्यक उपकरण:
लोहे की बॉल मिल
एथेनॉल - प्रयोगशाला श्रेणी, 95 %
सुखाने की भट्ठी
P100 श्वासयंत्र5
5
Press discs at 1.5 tons per cm²
Press discs at 1.5 tons per cm²
Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).
आवश्यक उपकरण:
हाइड्रोलिक प्रेस
डिस्क दबाने की डाई6
6
Sinter 4 hours at 1200 °C
Sinter 4 hours at 1200 °C
Sinter the discs for 4 hours at 1200 °C in oxygen or in air. The patent's strontium rod at 1200 °C: 1,340 gauss and 3,900 oersted.
आवश्यक उपकरण:
मफल भट्ठी
क्रूसिबल चिमटा
ताप-रोधी दस्ताने7
7
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
आवश्यक उपकरण:
विद्युत-चुंबक
दिक्सूचकसामग्री
2- 29.5 ग्राप्लेसहोल्डर
- 191.7 ग्राप्लेसहोल्डर
आवश्यक उपकरण
14- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
यह ब्लूप्रिंट बनाता है
संबंधित ब्लूप्रिंट
ये ब्लूप्रिंट ज्ञान साझा करते हैं — तकनीक, सामग्री या सिद्धांत

Barium Ferrite Disc Magnet: Barium Carbonate and Iron Oxide Sintered (Went, Philips 1956)
Charlie द्वारा
औद्योगिक
5
0
0
0
0
0

Strontium Carbonate: Powdered Celestine Boiled with Soda Solution (Thorpe 1912)
Charlie द्वारा
औद्योगिक
9
0
0
0
0
0

खतरनाक
Ferrite Toroid Core: Nickel-Zinc Ferrite Sintered at 1300 °C in Oxygen (Snoek)
Charlie द्वारा
औद्योगिक
15
0
0
0
0
0

Ferric Oxide: Hydroxide Precipitated from Ferric Chloride with Ammonia, Then Heated
Charlie द्वारा
अकार्बनिक
11
0
0
0
0
0
CC0 पब्लिक डोमेन
यह ब्लूप्रिंट CC0 के तहत जारी किया गया है। आप बिना अनुमति माँगे इस कार्य को किसी भी उद्देश्य के लिए कॉपी, संशोधित, वितरित और उपयोग करने के लिए स्वतंत्र हैं।
उनके ब्लूप्रिंट के माध्यम से उत्पाद खरीदकर मेकर का समर्थन करें जहाँ वे मेकर कमीशन कमाते हैं जो विक्रेताओं द्वारा निर्धारित होता है, या इस ब्लूप्रिंट का नया संस्करण बनाएँ और राजस्व साझा करने के लिए इसे अपने ब्लूप्रिंट में कनेक्शन के रूप में शामिल करें।