Thread Locker: Tetraethylene Glycol Dimethacrylate with Cumene Hydroperoxide, Set When Air Is Shut Out (Krieble, US 2,895,950)
Charlie

द्वारा बनाया गया

Charlie

2. नवंबर 2026DE
1
0
0
0
0

Thread Locker: Tetraethylene Glycol Dimethacrylate with Cumene Hydroperoxide, Set When Air Is Shut Out (Krieble, US 2,895,950)

An anaerobic thread locker. A little cumene hydroperoxide stirred into tetraethylene glycol dimethacrylate stays liquid as long as air reaches it. Shut between threads or plates, away from air, it sets into a tough resin and locks them. Result: a liquid that keeps a year or more in a half-full bottle and locks steel in 40 minutes to 5 hours, depending on how much catalyst it holds. Heat speeds it up. Source: V. K. Krieble (American Sealants Company), US 2,895,950 (1959), Example 1. Unknown: how the tetraethylene glycol dimethacrylate is made; the patent uses a bought commercial grade. Not given: bond strength. Picture: Wikimedia Commons.
शुरुआती
2 hours

निर्देश

1

Mix in the catalyst

At room temperature, stir cumene hydroperoxide into commercial-grade tetraethylene glycol dimethacrylate, measuring by volume. Anything from 0.1 to 10 % works; the patent prefers 2 to 10 %. Goggles and gloves: cumene hydroperoxide is an organic peroxide, keep it cool.

इस चरण के लिए सामग्री:

टेट्राएथिलीन ग्लाइकॉल डाइमेथैक्रिलेटटेट्राएथिलीन ग्लाइकॉल डाइमेथैक्रिलेट100 parts by volume
क्यूमीन हाइड्रोपरऑक्साइडक्यूमीन हाइड्रोपरऑक्साइड5 parts by volume (0.1-10)

आवश्यक उपकरण:

मापन सिलिंडरमापन सिलिंडर
हिलाने वाली छड़हिलाने वाली छड़
बंद सुरक्षा चश्माबंद सुरक्षा चश्मा
रसायन-रोधी दस्तानेरसायन-रोधी दस्ताने
2

Store it with air

Keep the mixture in a container with air space, preferably polyethylene, which lets air through. Bottles stored half full stayed liquid for a year or more at room temperature.

आवश्यक उपकरण:

प्लास्टिक की बोतलप्लास्टिक की बोतल
3

Apply to the threads

Put a few drops on the threads before joining the parts. Once air is shut out it sets. Average set times between steel plates at 25-27 °C, by catalyst share: 10 %, 42 min; 5 %, 52 min; 2 1/2 %, 74 min; 1 1/4 %, 84 min. With 0.1 % it takes about five hours.

आवश्यक उपकरण:

पिपेट और ड्रॉपर सेटपिपेट और ड्रॉपर सेट
4

Speed it up with heat

Heat sets it faster: the 0.1 % mixture between glass slides, warmed to 100 °C over a steam bath, locked them in five minutes. Ours: a water bath over a burner as the steam bath.

आवश्यक उपकरण:

जल-स्नानजल-स्नान
बुन्सन बर्नरबुन्सन बर्नर

सामग्री

2

आवश्यक उपकरण

8

यह ब्लूप्रिंट बनाता है

संबंधित ब्लूप्रिंट

ये ब्लूप्रिंट ज्ञान साझा करते हैं — तकनीक, सामग्री या सिद्धांत

CC0 पब्लिक डोमेन

यह ब्लूप्रिंट CC0 के तहत जारी किया गया है। आप बिना अनुमति माँगे इस कार्य को किसी भी उद्देश्य के लिए कॉपी, संशोधित, वितरित और उपयोग करने के लिए स्वतंत्र हैं।

उनके ब्लूप्रिंट के माध्यम से उत्पाद खरीदकर मेकर का समर्थन करें जहाँ वे मेकर कमीशन कमाते हैं जो विक्रेताओं द्वारा निर्धारित होता है, या इस ब्लूप्रिंट का नया संस्करण बनाएँ और राजस्व साझा करने के लिए इसे अपने ब्लूप्रिंट में कनेक्शन के रूप में शामिल करें।

चर्चा

(0)

लॉग इन करें चर्चा में शामिल होने के लिए

टिप्पणियाँ लोड हो रही हैं...