Ytterbium: Oxide Reduced by Lanthanum at 1020 °C in Vacuum, Metal Distilled Off (Shindo and Yagi, US 2010/0260640)
Ytterbium boils far more easily than lanthanum. Heated with lanthanum in a vacuum, ytterbium oxide gives up its oxygen to the lanthanum, and the freed ytterbium leaves as vapour and condenses in a cooler zone, while lanthanum oxide stays behind.
Result: ytterbium metal ingots; 20 kg of distillate in the patent's run, low in sodium, potassium and lithium.
Source: Y. Shindo and K. Yagi, US patent application 2010/0260640 (2010), Example 1. Not given: how much lanthanum, the vacuum, the time, crucible and condenser materials. Picture drawn by Youblob.
उन्नत
1 day
निर्देश
1
1
Mix the oxide with lanthanum
Mix the oxide with lanthanum
Mix ytterbium oxide with lanthanum metal as the reducing agent. Not given: the proportions.
इस चरण के लिए सामग्री:
इटर्बियम ऑक्साइड1 as requiredआवश्यक उपकरण:
लैंथेनम
टैंटलम क्रूसिबल2
2
Reduce in vacuum at 1020 °C
Reduce in vacuum at 1020 °C
Heat the charge in a vacuum to 1020 °C: Yb2O3 + 2 La -> 2 Yb (vapour) + La2O3. Ours: a vacuum induction furnace; the vacuum level and time are not given.
आवश्यक उपकरण:
प्रेरण भट्ठी
निर्वात पंप
टैंटलम क्रूसिबल3
3
Condense the ytterbium at 200-600 °C
Condense the ytterbium at 200-600 °C
Catch the ytterbium vapour on a condenser held at 200-600 °C. Most of it settles in the 300-500 °C part; the 200-300 °C part carries the least sodium and lithium. Ours: a tantalum condenser plate.
आवश्यक उपकरण:
टैंटलम संघनक प्लेट4
4
Melt into ingots under argon
Melt into ingots under argon
Take the distillate off the condenser, melt it in a crucible at 950 °C under a slight pressure of argon, and let it solidify into an ingot.
आवश्यक उपकरण:
टैंटलम क्रूसिबल
प्रेरण भट्ठी
आर्गनसामग्री
1- 1 as requiredप्लेसहोल्डर
यह ब्लूप्रिंट बनाता है
संबंधित ब्लूप्रिंट
ये ब्लूप्रिंट ज्ञान साझा करते हैं — तकनीक, सामग्री या सिद्धांत

खतरनाक
Erbium, Ytterbium, Thulium and Lutetium Oxides: Xenotime Separated on Ion Exchange Columns with EDTA and HEDTA (Spedding and Powell, US 2,956,858)
Charlie द्वारा
अकार्बनिक
2
0
0
0
0
0

खतरनाक
Lanthanum: Anhydrous Chloride Reduced with Calcium in a Tantalum Bomb under Argon, then Vacuum Cast (Daane, Ames 1950)
Charlie द्वारा
अकार्बनिक
1
0
0
0
0
0
CC0 पब्लिक डोमेन
यह ब्लूप्रिंट CC0 के तहत जारी किया गया है। आप बिना अनुमति माँगे इस कार्य को किसी भी उद्देश्य के लिए कॉपी, संशोधित, वितरित और उपयोग करने के लिए स्वतंत्र हैं।
उनके ब्लूप्रिंट के माध्यम से उत्पाद खरीदकर मेकर का समर्थन करें जहाँ वे मेकर कमीशन कमाते हैं जो विक्रेताओं द्वारा निर्धारित होता है, या इस ब्लूप्रिंट का नया संस्करण बनाएँ और राजस्व साझा करने के लिए इसे अपने ब्लूप्रिंट में कनेक्शन के रूप में शामिल करें।