Barium Sulphide: Heavy Spar Roasted with Coal
Barium sulphide is the barium half of lithopone, the white pigment. Thorpe (1912): roast 100 parts of heavy spar with 20 parts of coal slack or charcoal. Caking bituminous coal soaks through the mass and reduces it completely; with charcoal, mix very thoroughly. The roasted mass still holds carbon and some unchanged spar: hot water takes out the barium sulphide. Left in air it turns to carbonate and smells of rotten eggs, so keep it closed.
The picture: our own drawing.
متوسط
1 day
دستورالعملها
1
1
Grind and mix
Grind and mix
Grind 100 g of heavy spar and 20 g of bituminous coal slack and mix them very thoroughly.
مواد مورد نیاز این مرحله:
باریت (اسپار سنگین)100 گرمابزارهای مورد نیاز:
زغالسنگ قیری
هاون و دستهٔ هاون
ترازوی دو کفه2
2
Roast
Roast
Roast the mixture in a crucible in the furnace. The coal cakes and runs through the mass, reducing the spar.
ابزارهای مورد نیاز:
بوتهٔ گِلی عمیق
کورهٔ زغالچوبی
دستکش چرمی3
3
Cool and close it up
Cool and close it up
Let it cool and put it straight into an airtight jar. It holds spare carbon and some unchanged spar; hot water dissolves out the barium sulphide when you use it.
ابزارهای مورد نیاز:
شیشههای تیره با درِ هوابند
دستکش چرمیمواد
1- 100 گرمجایگزین
ابزارهای لازم
7- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
این نقشه میسازد
CC0 مالکیت عمومی
این نقشه تحت مجوز CC0 منتشر شده است. شما آزاد هستید آن را کپی، ویرایش، توزیع و برای هر هدفی بدون نیاز به اجازه استفاده کنید.
با خرید محصولات از طریق نقشه از سازنده حمایت کنید و او کمیسیون سازنده تعیین شده توسط فروشندگان، دریافت میکند یا یک نسخه جدید از این نقشه ایجاد کنید و آن را به عنوان اتصال در نقشه خود قرار دهید تا درآمد به اشتراک گذاشته شود.