Epoxy Resin
Woody

ایجاد شده توسط

Woody

22. سپتامبر 2026NO
۱
۰
۰
۰
۰

Epoxy Resin

Pierre Castan, a Swiss chemist at the dental firm De Trey Frères, was looking for a resin for dentures. He reacted a phenol carrying two hydroxy groups with epichlorohydrin, then hardened the product with an acid anhydride, and got a hard, clear, unusually adherent solid. Ciba licensed it and sold it as Araldite; in the US Sylvan Greenlee developed epoxies independently. **US 2,324,483**, "Process of preparing synthetic resins", Castan, granted 20. July 1943, claims condensing "a polybasic carboxylic acid anhydride" with the product of "a phenol having at least two phenolic hydroxy groups and of an epichlorhydrine". It does not single out bisphenol A, the phenol most epoxies use today. **Epichlorohydrin is a carcinogen; you start from a two-part kit.** You glue pine lap joints at the right ratio and four wrong ones, then test hardness and break the joints.
مبتدی
2 hours plus 24 h cure

دستورالعمل‌ها

1

Cut the joint pieces

Saw ten pine strips 100 x 25 mm. Sand one face of each end with 120 grit and dust off. Label five pairs 1:1, 1.25:1, 1:1.25, 1.5:1 and 1:1.5.

مواد مورد نیاز این مرحله:

تختهٔ کاجتختهٔ کاج1 قطعه
کاغذ سنبادهکاغذ سنباده1 ورق
چسب نواری کاغذیچسب نواری کاغذی1 رول

ابزارهای مورد نیاز:

ارهٔ دستیارهٔ دستی
خط‌کش فولادیخط‌کش فولادی
مدادمداد
2

Measure by syringe

Gloves on. For each ratio draw resin and hardener in separate syringes (1:1 = 2 ml + 2 ml; 1.25:1 = 2.5 + 2; and so on) into its own cup. This assumes a 1:1-by-volume kit - scale to your label.

مواد مورد نیاز این مرحله:

اپوکسی دوجزئیاپوکسی دوجزئی25 میلی‌لیتر

ابزارهای مورد نیاز:

دستکش نیتریلدستکش نیتریل
مجموعهٔ سرنگمجموعهٔ سرنگ
پیمانه‌های هم‌زدن مدرّجپیمانه‌های هم‌زدن مدرّج
عینک ایمنی شفافعینک ایمنی شفاف
3

Mix thoroughly

Stir each cup 2 minutes, scraping the walls and bottom. Unmixed streaks behave like a wrong ratio.

ابزارهای مورد نیاز:

همزنهمزن
4

Glue and pour

Spread each mix on the sanded ends of its pair, overlap them 25 mm and spring-clamp over wax paper. Pour the rest as a coin-sized puddle on wax paper beside it.

مواد مورد نیاز این مرحله:

کاغذ مومیکاغذ مومی1 ورق

ابزارهای مورد نیاز:

گیرهٔ فنریگیرهٔ فنری
5

Cure 24 hours

Leave everything at room temperature, 20 °C or warmer, for 24 hours. Cold slows the cure.
6

Pencil hardness

Sharpen pencils 6B to 6H and flatten the tips on 400 grit. Push each at 45° across a puddle, from hard down, until one no longer scratches. Record that grade.

ابزارهای مورد نیاز:

مجموعه مداد گرافیتیمجموعه مداد گرافیتی
ذره‌بین جواهرسازیذره‌بین جواهرسازی
7

Break the joints

Clamp one strip of a joint in the vise and tap the free end sideways with the mallet until it breaks. Estimate how much of the bond face is torn wood.

ابزارهای مورد نیاز:

گیرهٔ رومیزیگیرهٔ رومیزی
چکش لاستیکیچکش لاستیکی
عینک ایمنی شفافعینک ایمنی شفاف
8

Ratio, leftovers, results

در حال بارگذاری دفترچهٔ Jupyter…
9

History & Context

**What the patent specifies:** a resin from a two-hydroxy phenol and epichlorohydrin, hardened by a polybasic acid anhydride. **Modern build (derived):** a two-part kit, most with an amine hardener that cures at room temperature. Epoxy became the glue that holds metal, the matrix of fibreglass and carbon-fibre parts, and the boat-builder's resin. Its limits: it yellows in sunlight, softens with heat, and uncured resin and hardener sensitise skin - which is why the gloves stay on every time.

مواد

5

ابزارهای لازم

13

CC0 مالکیت عمومی

این نقشه تحت مجوز CC0 منتشر شده است. شما آزاد هستید آن را کپی، ویرایش، توزیع و برای هر هدفی بدون نیاز به اجازه استفاده کنید.

با خرید محصولات از طریق نقشه از سازنده حمایت کنید و او کمیسیون سازنده تعیین شده توسط فروشندگان، دریافت می‌کند یا یک نسخه جدید از این نقشه ایجاد کنید و آن را به عنوان اتصال در نقشه خود قرار دهید تا درآمد به اشتراک گذاشته شود.

بحث و گفتگو

(0)

ورود برای شرکت در بحث

در حال بارگذاری نظرات...