Forged Hunting Axe (Hatchet)
Forge

ایجاد شده توسط

Forge

11. اکتبر 2026NO
۳۲
۰
۰
۰
۰

Forged Hunting Axe (Hatchet)

A small one-handed axe forged from a 7/8 × 2-inch bar of good tool steel, best made by two people; a 6¾-inch bar gives two heads. The eye, about 9/16 × 1½ inches, is punched at a yellow heat with an eye punch and opened with drifts, the blade drawn out to a 3-inch edge and the head cut to length. The axe is annealed in lime or ashes, ground and buffed, then hardened from the hardening heat in tepid water and tempered by two hot iron bars laid on either side at the centre: dark purple for the blade, blue for the head.
پیشرفته
4–6 hours

دستورالعمل‌ها

1

Mark and punch the eye

Mark the stock with chisel and centre punch. At a yellow heat, punch the eye with the narrow edge of the punch toward the blade; lift the punch after each blow to check it runs straight and to let it cool; a little fine coal in the hole stops it sticking. Punch nearly through, then finish from the other side.

مواد مورد نیاز این مرحله:

تسمهٔ فولاد ابزارتسمهٔ فولاد ابزار1 قطعه

ابزارهای مورد نیاز:

سنبهٔ نشانه‌گذاریسنبهٔ نشانه‌گذاری
کورهٔ آهنگریکورهٔ آهنگری
سندانسندان
سنبهٔ داغسنبهٔ داغ
پتکپتک
انبر آهنگریانبر آهنگری
2

Drift and draw out

Drive in a tool-steel drift, hammer the bulges down to the bar's size and smooth with a flatter; take the drift out before each reheat. Use two drifts, the first 3/8 inch narrower. Draw out the blade, driving the drift back in as the eye stretches so no cold shut forms.

ابزارهای مورد نیاز:

سنبه گشادکن سوراخسنبه گشادکن سوراخ
ابزار تخت‌کنابزار تخت‌کن
پتک بادامکیپتک بادامکی
3

Shape and trim

Shape the blade with a heavy hammer and flatter and form its edge. Cut the head from the bar, draw it to size, cut it to length, then trim the blade to shape.

ابزارهای مورد نیاز:

چکش آهنگریچکش آهنگری
ابزار تخت‌کنابزار تخت‌کن
قلم داغقلم داغ
4

Anneal and grind

Heat to a full red and anneal in lime or ashes. When cold, grind on an emery wheel and finish on a buffing wheel.

ابزارهای مورد نیاز:

کورهٔ آهنگریکورهٔ آهنگری
سنگ‌سنبادهٔ رومیزیسنگ‌سنبادهٔ رومیزی
5

Harden and temper

Heat very slowly to the hardening heat and cool in tepid water. Draw the temper with two hot iron bars laid on either side at the centre; when the blade is dark purple and the head blue, cool quickly in water.

ابزارهای مورد نیاز:

کورهٔ آهنگریکورهٔ آهنگری
سطل آب‌دهیسطل آب‌دهی
انبر آهنگریانبر آهنگری
6

Handle

Shave the handle stock to fit the eye tightly, drive the head on, saw a kerf in the handle's top and drive a glued hardwood wedge into it. Trim flush and oil the handle.

مواد مورد نیاز این مرحله:

چوب سخت برای دستهچوب سخت برای دسته1 قطعه
گُوِهٔ چوب سختگُوِهٔ چوب سخت1 قطعه
روغن بزرکروغن بزرک10 میلی‌لیتر

ابزارهای مورد نیاز:

رندهٔ دودستهرندهٔ دودسته
اره دونفره عرض‌براره دونفره عرض‌بر
گیرهٔ رومیزیگیرهٔ رومیزی

مواد

4

ابزارهای لازم

16

این نقشه می‌سازد

نقشه‌های مرتبط

این نقشه‌ها دانش مشترکی دارند — تکنیک‌ها، مواد یا اصول

CC0 مالکیت عمومی

این نقشه تحت مجوز CC0 منتشر شده است. شما آزاد هستید آن را کپی، ویرایش، توزیع و برای هر هدفی بدون نیاز به اجازه استفاده کنید.

با خرید محصولات از طریق نقشه از سازنده حمایت کنید و او کمیسیون سازنده تعیین شده توسط فروشندگان، دریافت می‌کند یا یک نسخه جدید از این نقشه ایجاد کنید و آن را به عنوان اتصال در نقشه خود قرار دهید تا درآمد به اشتراک گذاشته شود.

بحث و گفتگو

(0)

ورود برای شرکت در بحث

در حال بارگذاری نظرات...