Rasps: Teeth Raised One at a Time with a Pointed Punch
Forge

ایجاد شده توسط

Forge

11. اکتبر 2026NO
۳۳
۰
۰
۰
۰

Rasps: Teeth Raised One at a Time with a Pointed Punch

A rasp is a coarse file whose teeth stand separately instead of in continuous rows. Each tooth is raised by driving a pointed punch into the face of the blank at uniform distances. Because the teeth stand apart, a rasp clogs less than a cut file on soft material such as wood or a horse's hoof. The blank is forged, annealed and ground like a file blank, and the finished rasp is hardened like a file: coated against scale, brought to a dull red heat and plunged into water, with the tang tempered so it will not snap. Machine-made rasps have uniformly stamped teeth, which line up row behind row and leave deeper marks; slightly uneven hand-cut teeth avoid this.
پیشرفته
2 days (annealing overnight)

دستورالعمل‌ها

1

Forge the blank

Forge the steel to a tapered bar, flat, round or half-round, with a narrow pointed tang at one end.

مواد مورد نیاز این مرحله:

شمش فولاد پرکربنشمش فولاد پرکربن0.5 کیلوگرم

ابزارهای مورد نیاز:

کورهٔ آهنگریکورهٔ آهنگری
سندانسندان
چکش آهنگریچکش آهنگری
انبر آهنگریانبر آهنگری
2

Anneal and grind

Anneal the blank soft so the teeth can be raised, then grind the faces to a smooth, clear surface.

ابزارهای مورد نیاز:

کورهٔ آهنگریکورهٔ آهنگری
سنگ چرخان تیزکنیسنگ چرخان تیزکنی
3

Punch the teeth

Drive the pointed punch into the face with the hammer at uniform distances, raising one separate tooth at each blow. Turn the rasp over on a soft metal plate to work the other face without crushing the finished teeth.

ابزارهای مورد نیاز:

سنبهٔ سوهان زبرسنبهٔ سوهان زبر
چکش آهنگریچکش آهنگری
سندانسندان
صفحهٔ پیوترصفحهٔ پیوتر
4

Harden

Coat the toothed surface thickly with a salt composition against scaling, raise the rasp to a dull red heat in a clear coke fire and plunge it upright into water. If it bends, straighten it across a fulcrum before it is fully cold.

مواد مورد نیاز این مرحله:

نمکنمک1 کیلوگرم
کک متالورژیکک متالورژی1 as required

ابزارهای مورد نیاز:

کورهٔ آهنگریکورهٔ آهنگری
سطلسطل
انبر آهنگریانبر آهنگری
5

Temper the tang and clean

Temper the tang by dipping it in molten lead so it will not snap. Scour and wash off every trace of salt, then brush the rasp with oil.

ابزارهای مورد نیاز:

حمام سرب مذابحمام سرب مذاب
انبر آهنگریانبر آهنگری

مواد

3
  • جایگزین
  • 1 کیلوگرم
    جایگزین
  • جایگزین

ابزارهای لازم

9

CC0 مالکیت عمومی

این نقشه تحت مجوز CC0 منتشر شده است. شما آزاد هستید آن را کپی، ویرایش، توزیع و برای هر هدفی بدون نیاز به اجازه استفاده کنید.