PETG Pellets: Dimethyl Terephthalate with Ethylene Glycol and CHDM
PETG is PET in which part of the ethylene glycol is replaced by CHDM, which keeps the plastic clear and amorphous. Eastman's patent US 7,026,027 describes PETG 6763 as terephthalate with about 69 mol % ethylene glycol and 31 mol % CHDM, but gives no recipe for it. This blueprint is our own combination: that composition, made by the same patent's pilot-plant process (Example 12, written for a CHDM/neopentyl glycol copolyester), with ethylene glycol in place of neopentyl glycol as in Kibler's 1959 Eastman patent. The charge weights are our arithmetic.
The picture: our diagram.
پیشرفته
About 5 hours
دستورالعملها
1
1
Charge the reactor
Charge the reactor
Our charge for 31 mol % CHDM: 10.669 kg dimethyl terephthalate (54.9 mol, as in the patent's example), 2.456 kg CHDM (31 % of those moles) and 4.058 kg ethylene glycol, so the glycols total 1.5 times the ester moles as in the example. Add 53.4 g of catalyst solution (15 g titanium isopropoxide in 250 ml n-butanol). The patent's reactor held 18 gallons and had spiral agitators and a distillation column.
مواد مورد نیاز این مرحله:
دیمتیل ترفتالات10.669 کیلوگرم
1،4-سیکلوهگزاندیمتانول2.456 کیلوگرم
اتیلن گلیکول4.058 کیلوگرمابزارهای مورد نیاز:
تیتانیم ایزوپروپوکسید
نرمال بوتانول
ترازوی دو کفه
راکتور پلیمریزاسیون ژاکتدار
دیگ تقطیر جزءبهجزء
عینک محافظ در برابر پاشش مواد شیمیایی2
2
Ester interchange at 200 °C
Ester interchange at 200 °C
Stir (forward 50 minutes, then reverse 10), heat to 200 °C and hold 2 hours. Methanol distils off through the column.
ابزارهای مورد نیاز:
راکتور پلیمریزاسیون ژاکتدار
دیگ تقطیر جزءبهجزء
ترموکوپل با نمایشگر3
3
260 °C, then 280 °C
260 °C, then 280 °C
Raise to 260 °C for 30 minutes and weigh the distillate, then raise to 280 °C and weigh it again. The surplus ethylene glycol is driven off; Kibler found the CHDM stays in the polymer.
ابزارهای مورد نیاز:
راکتور پلیمریزاسیون ژاکتدار
ترموکوپل با نمایشگر
ترازوی دو کفه4
4
Polymerise under vacuum
Polymerise under vacuum
Switch the agitator direction every 6 minutes and pull vacuum at 13 Torr a minute down to 0.5 Torr. Hold full vacuum for 45 minutes at 25 rpm.
ابزارهای مورد نیاز:
راکتور پلیمریزاسیون ژاکتدار
پمپ خلأ
خلأسنج
تله سرد5
5
Extrude and chop into pellets
Extrude and chop into pellets
Let nitrogen in, extrude the polymer at once and chop it into pellets. Check the composition: in the patent's example the polymer kept slightly less CHDM than was charged (38.1 % for 40.7 %).
ابزارهای مورد نیاز:
کپسول گاز نیتروژن
دانهساز
دستکش گرمااستوارمواد
3- 10.669 کیلوگرمجایگزین
- 2.456 کیلوگرمجایگزین
- 4.058 کیلوگرمجایگزین
ابزارهای لازم
13- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- 1 vendor sell this, none ship to you yetجایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
این نقشه میسازد
نقشههای مرتبط
این نقشهها دانش مشترکی دارند — تکنیکها، مواد یا اصول

خطرناک
1,4-Cyclohexanedimethanol: Dimethyl Terephthalate Hydrogenated over Palladium, then Copper Chromite
توسط Charlie
صنعتی
۱۲
۰
۰
۰
۰
۰

Dimethyl Terephthalate: Terephthalic Acid and Methanol Sprayed through a Hot Tube
توسط Charlie
صنعتی
۱۰
۰
۰
۰
۰
۰

خطرناک
Ethylene Glycol by Hydration of Ethylene Oxide
توسط Charlie
صنعتی
۶
۰
۰
۰
۰
۰
CC0 مالکیت عمومی
این نقشه تحت مجوز CC0 منتشر شده است. شما آزاد هستید آن را کپی، ویرایش، توزیع و برای هر هدفی بدون نیاز به اجازه استفاده کنید.
با خرید محصولات از طریق نقشه از سازنده حمایت کنید و او کمیسیون سازنده تعیین شده توسط فروشندگان، دریافت میکند یا یک نسخه جدید از این نقشه ایجاد کنید و آن را به عنوان اتصال در نقشه خود قرار دهید تا درآمد به اشتراک گذاشته شود.