Polypropylene Felt: a Spunbonded Web, Kinney 1967

A polypropylene felt made without weaving or needling: hot filaments are spun, pulled down by an air jet, given an electric charge so they spread apart, and laid in loops on a moving table until they form an even sheet. Kinney's patent (Du Pont, US 3,338,992, 1967) gives every setting for polypropylene. The corona runs at 20 to 25 kV: keep clear of it while it is live. The picture: the patent's own Fig. 1 (the process) and Fig. 7 (the web).
پیشرفته
1 day

دستورالعمل‌ها

1

Melt and spin

Melt polypropylene of melt index 10 in a screw extruder, no hotter than 290 °C. Meter it at 12 g a minute through a 1/4 in. sand filter and a 20-hole spinneret (holes 0.015 in. across): pack block 275 °C, spinneret 260 °C.

مواد مورد نیاز این مرحله:

گرانول پلی‌پروپیلنگرانول پلی‌پروپیلن500 گرم

ابزارهای مورد نیاز:

اکسترودر پلاستیکاکسترودر پلاستیک
رشته‌ساز (اسپینرت)رشته‌ساز (اسپینرت)
پیرومترپیرومتر
ترازوی دو کفهترازوی دو کفه
دستکش چرمیدستکش چرمی
2

Quench

Cool the bundle of filaments in a 6 in. quench chimney blowing 40 cubic feet a minute of room air in from the side.

ابزارهای مورد نیاز:

کمپرسور هواکمپرسور هوا
3

Draw with the air jet

Lead the bundle 72 in. down into an air draw jet run at 25 psi: it pulls the filaments with about 3 g of tension and stretches them.

ابزارهای مورد نیاز:

نازل کشش هوایینازل کشش هوایی
کمپرسور هواکمپرسور هوا
فشارسنجفشارسنج
4

Charge the filaments

8 in. above the jet, let the filaments brush a 1 1/4 in. bar turning at 10 rpm, with a four-point corona 5/8 in. from it at minus 20 to 25 kV (100 to 150 µA). The charge pushes them apart. Keep clear while it is live.

ابزارهای مورد نیاز:

واحد شارژ کروناواحد شارژ کرونا
5

Lay the web

Catch the filaments on a grounded 47 in. square table that moves 26 in. a minute one way and 570 in. a minute the other. Each layer weighs 0.5 oz per square yard; lay several for each sheet.

ابزارهای مورد نیاز:

میز انباشتمیز انباشت
6

What you get

An even sheet of fine filaments, about 2.5 denier each, tenacity 2.0 g per denier, stretching 300 % before they break.

ابزارهای مورد نیاز:

ترازوی دو کفهترازوی دو کفه

مواد

1

ابزارهای لازم

10

CC0 مالکیت عمومی

این نقشه تحت مجوز CC0 منتشر شده است. شما آزاد هستید آن را کپی، ویرایش، توزیع و برای هر هدفی بدون نیاز به اجازه استفاده کنید.

با خرید محصولات از طریق نقشه از سازنده حمایت کنید و او کمیسیون سازنده تعیین شده توسط فروشندگان، دریافت می‌کند یا یک نسخه جدید از این نقشه ایجاد کنید و آن را به عنوان اتصال در نقشه خود قرار دهید تا درآمد به اشتراک گذاشته شود.

بحث و گفتگو

(0)

ورود برای شرکت در بحث

در حال بارگذاری نظرات...