Neodymium Magnets, Sample 21: 75Fe-8B-17Nd Sintered (Sagawa 1988)
Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 21, 75 % iron, 8 % boron and 17 % neodymium by atoms: 31.1 MGOe.
Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made, and how the finished magnets are magnetised; the patent does not say. The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
متخصص
2 days
دستورالعملها
1
1
Weigh sample 21: 75 Fe, 8 B, 17 Nd
Weigh sample 21: 75 Fe, 8 B, 17 Nd
Sample 21 is 75 % iron, 8 % boron and 17 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 573.2 g iron, 66.3 g ferroboron, 364.5 g neodymium. Unknown: how these three are made.
مواد مورد نیاز این مرحله:
آهن الکترولیتی573.2 گرم
فروبور66.3 گرم
فلز نئودیمیم364.5 گرمابزارهای مورد نیاز:
ترازوی دو کفه2
2
Melt by high frequency in argon and cast
Melt by high frequency in argon and cast
Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.
ابزارهای مورد نیاز:
کورهٔ القایی
بوتهٔ گِل نسوز
آرگون
کپسول گاز تحت فشار
قالب مسی آبخنک
دستکش گرمااستوار3
3
Stamp to 35 mesh, ball-mill to 3-10 µm
Stamp to 35 mesh, ball-mill to 3-10 µm
Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.
ابزارهای مورد نیاز:
آسیاب کوبهای
مجموعهٔ الک (چشمهٔ پلکانی)
آسیاب گلولهای آهنی
عینک ایمنی4
4
Press in a 10 kOe field at 1.5 t/cm²
Press in a 10 kOe field at 1.5 t/cm²
Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.
ابزارهای مورد نیاز:
پرس با میدان مغناطیسی5
5
Sinter in argon at 1000-1200 °C
Sinter in argon at 1000-1200 °C
Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 21 measured 11.6 kG remanence, 9.2 kOe coercivity and 31.1 MGOe.
ابزارهای مورد نیاز:
کورهٔ لولهای
آرگون
کپسول گاز تحت فشار
دستکش گرمااستوار6
6
Magnetise the magnets
Magnetise the magnets
Unknown: how the sintered magnets are magnetised. Sagawa measures them on a B-H tracer but gives no magnetising field or apparatus.
ابزارهای مورد نیاز:
روش مغناطیسکردن ناشناختهمواد
3- 573.2 گرمجایگزین
- 66.3 گرمجایگزین
- 364.5 گرمجایگزین
ابزارهای لازم
14- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
نقشههای مرتبط
این نقشهها دانش مشترکی دارند — تکنیکها، مواد یا اصول
CC0 مالکیت عمومی
این نقشه تحت مجوز CC0 منتشر شده است. شما آزاد هستید آن را کپی، ویرایش، توزیع و برای هر هدفی بدون نیاز به اجازه استفاده کنید.
با خرید محصولات از طریق نقشه از سازنده حمایت کنید و او کمیسیون سازنده تعیین شده توسط فروشندگان، دریافت میکند یا یک نسخه جدید از این نقشه ایجاد کنید و آن را به عنوان اتصال در نقشه خود قرار دهید تا درآمد به اشتراک گذاشته شود.