Arthur F. Payne · Public domain (1914)
Teaspoon Forged from a Silver Bar (Payne 1914)
A 6-inch silver teaspoon forged out of a small bar of silver, the way a blacksmith forges iron. Arthur Payne called it the hardest of his five spoon methods, but the cheapest, because almost no silver is wasted.
Source: A. F. Payne, Art Metalwork with Inexpensive Equipment (1914), pp. 184–186; annealing from his chapter XI. Cutting the bar from sheet is ours. Picture: Payne's Fig. 158, teaspoons forged this way.
پیشرفته
1 day
دستورالعملها
1
1
Cut the silver bar
Cut the silver bar
For a teaspoon 6 in long you need a piece of sterling silver 4 in long, ½ in wide and ⅛ in thick. Mark it out and saw it from sheet of that thickness (cutting from sheet is ours).
مواد مورد نیاز این مرحله:
ورق نقره استرلینگ1 piece 4 × ½ × ⅛ inابزارهای مورد نیاز:
سوزن خطانداز
اره جواهرسازی2
2
Forge out the bowl
Forge out the bowl
Heat the bar until it is almost red-hot, hold it in tongs and forge the bowl out on the anvil. Silver forges more easily when it is nearly red, but never hammer it while it is red-hot: it will crack.
ابزارهای مورد نیاز:
چراغ بونزن
انبر
سندان
چکش3
3
Work bowl, then shank and handle
Work bowl, then shank and handle
Hammer the bowl until it is hard, then the shank and handle, so the whole spoon is hard before you anneal it again. That saves time.
ابزارهای مورد نیاز:
سندان
چکش4
4
Anneal and repeat
Anneal and repeat
To soften it, heat it to a dull red and plunge it into water, or let it cool. Then go on forging until the spoon is roughly to shape.
مواد مورد نیاز این مرحله:
آب1 as requiredابزارهای مورد نیاز:
چراغ بونزن
انبر
ظرف شیشهای5
5
Trim with shears and file
Trim with shears and file
Trim the outline with the shears and file the edges smooth.
ابزارهای مورد نیاز:
قیچی فلز سنگینکار
سوهان (سوهان دستی)6
6
Polish out the file marks
Polish out the file marks
Rub out all the scratches and file marks with emery cloth.
ابزارهای مورد نیاز:
پارچهٔ سنباده7
7
Anneal to even the fire scale
Anneal to even the fire scale
Anneal the spoon thoroughly once more. Heated silver grows a thin white skin, the fire scale, and this brings it back over the spots where filing and polishing took it off, so the colour is even.
مواد مورد نیاز این مرحله:
آب1 as requiredابزارهای مورد نیاز:
چراغ بونزن
انبر
ظرف شیشهای8
8
Planish with smooth hammers
Planish with smooth hammers
Planish the spoon on smooth tools with smooth, bright hammers. This makes it stiff again after the annealing.
ابزارهای مورد نیاز:
چکش پرداخت
سندان
میخ چوبی9
9
Final polish with rouge
Final polish with rouge
Polish it lightly with a soft cotton flannel and a little red rouge.
ابزارهای مورد نیاز:
پارچهٔ جلادهی جواهر
سرخاب زرگریابزارهای لازم
14- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
این نقشه میسازد
نقشههای مرتبط
این نقشهها دانش مشترکی دارند — تکنیکها، مواد یا اصول
CC0 مالکیت عمومی
این نقشه تحت مجوز CC0 منتشر شده است. شما آزاد هستید آن را کپی، ویرایش، توزیع و برای هر هدفی بدون نیاز به اجازه استفاده کنید.
با خرید محصولات از طریق نقشه از سازنده حمایت کنید و او کمیسیون سازنده تعیین شده توسط فروشندگان، دریافت میکند یا یک نسخه جدید از این نقشه ایجاد کنید و آن را به عنوان اتصال در نقشه خود قرار دهید تا درآمد به اشتراک گذاشته شود.