Metal Oxide Varistor: Pure Zinc Oxide at 1400 °C, Bismuth Oxide Paste Fired at 800 °C (Masuyama 1972, Ex. 4)
A varistor made the other way round: a disc of pure zinc oxide, sintered, with bismuth oxide fired into its faces from a paste instead of mixed in. Sintered at 1400 °C and fired with the paste at 800 °C, the disc measured a C-value of 85 at 1 mA and a nonlinearity exponent n of 7.2. Masuyama found that firing on the bismuth oxide paste raises n a great deal over mixing it in.
Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 4. Unknown: how the aluminium is sprayed on, what the silver paint is, and how strong the epoxy solution of the paste is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
پیشرفته
2 days
دستورالعملها
1
1
Press pure zinc oxide at 340 kg/cm²
Press pure zinc oxide at 340 kg/cm²
Press zinc oxide powder at 340 kg/cm². Example 4 gives no disc size; ours: discs 13 mm across and 2.5 mm thick in the mould of Example 1.
مواد مورد نیاز این مرحله:
پودر اکسید روی1 as requiredابزارهای مورد نیاز:
ترازوی دو کفه
پرس هیدرولیک
قالب پرس دیسک
کولیس ورنیه2
2
Sinter 1 hour at 1400 °C and cool
Sinter 1 hour at 1400 °C and cool
Heat the pressed disc for 1 hour at 1400 °C, then let it cool to room temperature.
ابزارهای مورد نیاز:
کوره مافل3
3
Lap both faces
Lap both faces
Lap both faces with silicon carbide abrasive. Example 4 gives no thickness.
ابزارهای مورد نیاز:
کولیس ورنیه4
4
Coat with bismuth oxide paste and fire at 800 °C
Coat with bismuth oxide paste and fire at 800 °C
Coat both lapped faces with a paste of 50 % by weight bismuth oxide in a solution of epoxy resin in butyl alcohol, and fire it in air at 800 °C for 30 minutes. The bismuth oxide diffuses into the zinc oxide. Not given: how much paste, or the strength of the epoxy solution.
مواد مورد نیاز این مرحله:
اکسید بیسموت1 as requiredابزارهای مورد نیاز:
رزین اپوکسی
نرمال بوتانول
کوره مافل5
5
Spray aluminium electrodes and attach leads
Spray aluminium electrodes and attach leads
Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint, as in Example 1. Unknown: the spraying method and the paint.
مواد مورد نیاز این مرحله:
شمش آلومینیوم1 as required
رنگ رسانای نقرهای1 as required
سیم مسی2 قطعهابزارهای مورد نیاز:
روش پاشش فلز نامعلوم
کولیس ورنیهمواد
5- 1 as requiredجایگزین
- 1 as requiredجایگزین
- 1 as requiredجایگزین
- 1 as requiredجایگزین
- 2 قطعهجایگزین
ابزارهای لازم
9- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
- جایگزین
این نقشه میسازد
نقشههای مرتبط
این نقشهها دانش مشترکی دارند — تکنیکها، مواد یا اصول
CC0 مالکیت عمومی
این نقشه تحت مجوز CC0 منتشر شده است. شما آزاد هستید آن را کپی، ویرایش، توزیع و برای هر هدفی بدون نیاز به اجازه استفاده کنید.
با خرید محصولات از طریق نقشه از سازنده حمایت کنید و او کمیسیون سازنده تعیین شده توسط فروشندگان، دریافت میکند یا یک نسخه جدید از این نقشه ایجاد کنید و آن را به عنوان اتصال در نقشه خود قرار دهید تا درآمد به اشتراک گذاشته شود.