Acrylic Block: Methyl Methacrylate Syrup Cast in Layers between Glass
Charlie

Búin til af

Charlie

20. október 2026DE
16
0
0
0
0

Acrylic Block: Methyl Methacrylate Syrup Cast in Layers between Glass

A thick acrylic block cannot be cast flawless in one pour. Tattersall (ICI, US 2,071,907, 1937) built it up in layers: pour 1/2 inch of syrup on a level glass plate, let it set for a day at room temperature, pour the next 1/2 inch on top, cover with a second glass plate, wait another day, then heat the sandwich at 80 °C. Each 1/2 inch layer shrinks to about 1/3 inch. The glass gives both faces a finished polish with no grinding. The picture: our diagram.
Miðlungs
3 days

Leiðbeiningar

1

Level the bottom plate

Set a glass plate on a ledge in a wooden frame, on a body of plaster of Paris, and level it carefully. The example sheet was 10 by 18 inches.

Nauðsynleg verkfæri:

GlerrúðaGlerrúða
TrérammiTrérammi
Gifs (Parísargifs)Gifs (Parísargifs)
HallamálHallamál
2

Pour the first 1/2 inch

Pour room-temperature syrup 1/2 inch deep (about 1.5 litres for 10 by 18 inches; our figure). Cover against dust, but do not put the top plate on yet. Leave 24 hours at about 20 °C.

Efni fyrir þetta skref:

MetýlmetakrýlatsírópMetýlmetakrýlatsíróp3 l

Nauðsynleg verkfæri:

GúmmíhanskarGúmmíhanskar
RannsóknastofuhitamælirRannsóknastofuhitamælir
3

Pour the next layer and cover

Pour a second 1/2 inch layer on the first. Lower the top glass plate onto it so it rests on the syrup and keeps pressing on it. Leave another 24 hours at about 20 °C. For a thicker block repeat the layers, a day apart, and put the plate on the last one.

Nauðsynleg verkfæri:

GlerrúðaGlerrúða
4

Heat at 80 °C

Take the glass sandwich out of the frame and heat it for three hours at 80 °C to finish the polymerisation.

Nauðsynleg verkfæri:

ÞurrkofnÞurrkofn
RannsóknastofuhitamælirRannsóknastofuhitamælir
Hitaþolnir hanskarHitaþolnir hanskar
5

Spring off the glass

Spring the glass plates off the block with a knife blade. Both faces come out smooth and polished.

Nauðsynleg verkfæri:

FöndurhnífurFöndurhnífur
GúmmíhanskarGúmmíhanskar

Efni

1

Nauðsynleg verkfæri

9

Tengd Blueprint

Þessi blueprint deila þekkingu — tækni, efni eða meginreglur

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...