Barium-Calcium Ferrite Disc Magnet: 20 % Calcium, 5 Minutes at 1290 °C (Went, Philips 1956, Ex. 20)
Charlie

Búin til af

Charlie

28. október 2026DE
2
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: 20 % Calcium, 5 Minutes at 1290 °C (Went, Philips 1956, Ex. 20)

A ceramic magnet with a fifth of the barium replaced by calcium: 0.08 mol barium carbonate, 0.02 mol calcium carbonate and 0.6 mol iron oxide, made as in Example 18 but sintered at 1290 °C for only 5 minutes. Went's rod held 1,615 gauss with a coercive force of 1,550 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 20. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lengra kominn
2 days

Leiðbeiningar

1

Weigh barium carbonate, chalk and iron oxide

Weigh 15.79 g barium carbonate (0.08 mol), 2.002 g calcium carbonate (0.02 mol) and 95.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Efni fyrir þetta skref:

Baríumkarbónat (witherít)Baríumkarbónat (witherít)15.79 g
Kalsíumkarbónat (kalkhvíta)Kalsíumkarbónat (kalkhvíta)2.002 g
Járn(III)oxíðJárn(III)oxíð95.55 g

Nauðsynleg verkfæri:

SkálavogSkálavog
GúmmíhanskarGúmmíhanskar
P100-öndunargrímaP100-öndunargríma
2

Mill, presinter and mill as in Example 18

As in Example 18: grind with alcohol 4 hours, dry at 150 °C, fire in air at 1000 °C for 2 hours, grind again 4 hours and dry.

Nauðsynleg verkfæri:

JárnkúlukvörnJárnkúlukvörn
Etanól - rannsóknargráða, 95 %Etanól - rannsóknargráða, 95 %
ÞurrkofnÞurrkofn
MúffluofnMúffluofn
Deigla með loki (postulín)Deigla með loki (postulín)
DeiglutöngDeiglutöng
3

Press at 1.5 t/cm²

Press at 1.5 tonnes per cm², as in Example 18 (ours: discs instead of rods).

Nauðsynleg verkfæri:

VökvapressaVökvapressa
Pressumót fyrir skífurPressumót fyrir skífur
4

Pass through a 1290 °C zone in 5 minutes

Sinter in air at 1290 °C by passing the pieces through a 10 cm hot zone at 20 mm per minute: 5 minutes in the heat.

Nauðsynleg verkfæri:

PípuofnPípuofn
Hitaþolnir hanskarHitaþolnir hanskar
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Nauðsynleg verkfæri:

RafmagnssegullRafmagnssegull
ÁttavitiÁttaviti

Efni

3

Nauðsynleg verkfæri

15

Tengd Blueprint

Þessi blueprint deila þekkingu — tækni, efni eða meginreglur

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.