Barium Ferrite Disc Magnet from Natural Magnetite, Presintered at 900 °C (Went, Philips 1956, Ex. 36, Procedure 1)

A barium ferrite magnet made from natural magnetite instead of ferric oxide: barium carbonate and magnetite ground 18 hours, presintered 3 hours at 900 °C, ground again 18 hours, pressed and sintered 2 hours at 1200 °C. Went's rod held 1,450 gauss with a coercive force of 2,425 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 36. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lengra kominn
2 days

Leiðbeiningar

1

Weigh barium carbonate and magnetite

Weigh 9.9 g barium carbonate (0.05 mol) and 46.9 g natural magnetite, Fe3O4 (0.20 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Efni fyrir þetta skref:

Baríumkarbónat (witherít)Baríumkarbónat (witherít)9.9 g
MagnetítMagnetít46.9 g

Nauðsynleg verkfæri:

SkálavogSkálavog
GúmmíhanskarGúmmíhanskar
P100-öndunargrímaP100-öndunargríma
2

Grind 18 hours in a ball mill

Grind the mixture in a ball mill for 18 hours. The patent does not say whether wet or dry.

Nauðsynleg verkfæri:

JárnkúlukvörnJárnkúlukvörn
P100-öndunargrímaP100-öndunargríma
3

Presinter at 900 °C for 3 hours

Fire the ground mixture at 900 °C for three hours and let it cool.

Nauðsynleg verkfæri:

MúffluofnMúffluofn
Deigla með loki (postulín)Deigla með loki (postulín)
DeiglutöngDeiglutöng
Hitaþolnir hanskarHitaþolnir hanskar
4

Grind 18 hours in a ball mill

Grind it again in a ball mill for 18 hours. The patent does not say whether wet or dry.

Nauðsynleg verkfæri:

JárnkúlukvörnJárnkúlukvörn
P100-öndunargrímaP100-öndunargríma
5

Press at 1.5 t/cm²

Press at 1.5 tonnes per cm² (ours: discs instead of a rod).

Nauðsynleg verkfæri:

VökvapressaVökvapressa
Pressumót fyrir skífurPressumót fyrir skífur
6

Sinter at 1200 °C for 2 hours

Sinter at 1200 °C for 2 hours. The patent gives no atmosphere for this example. Went's rod: 1,450 gauss, 2,425 oersted.

Nauðsynleg verkfæri:

MúffluofnMúffluofn
DeiglutöngDeiglutöng
Hitaþolnir hanskarHitaþolnir hanskar
7

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Nauðsynleg verkfæri:

RafmagnssegullRafmagnssegull
ÁttavitiÁttaviti

Efni

2

Nauðsynleg verkfæri

12

Tengd Blueprint

Þessi blueprint deila þekkingu — tækni, efni eða meginreglur

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...