Bearing Steel Wire (52100): Drawn from Bar Through a Drawplate
Forge

Búin til af

Forge

18. október 2026NO
14
0
0
0
0

Bearing Steel Wire (52100): Drawn from Bar Through a Drawplate

Bearing balls are headed from thick wire of 52100 steel. Here 52100 bar is forged to rod and drawn through a drawplate. At 1 % carbon it is much harder than mild steel, so it is annealed soft before drawing and again after every two holes, using the 52100 anneal Verhoeven recommends. The picture: our drawing, bar to coil.
Lengra kominn
2 days

Leiðbeiningar

1

Forge to rod

Heat the bar to a cherry-red heat and no hotter, and draw it out round on the anvil to a rod a little thicker than the drawplate's largest hole.

Efni fyrir þetta skref:

Legustálstöng (52100)Legustálstöng (52100)1 kg
ViðarkolViðarkol1 as required

Nauðsynleg verkfæri:

SmiðjueldstæðiSmiðjueldstæði
SteðjiSteðji
ÞverfleygshamarÞverfleygshamar
JárnsmiðstöngJárnsmiðstöng
SuðuhanskarSuðuhanskar
ÖryggisglerauguÖryggisgleraugu
2

Anneal

In the oven, hold it at 793 °C (1460 °F) for 30 minutes, cool in the oven no faster than 500 °C an hour to 682 °C (1260 °F), then cool in air.

Nauðsynleg verkfæri:

HitameðferðarofnHitameðferðarofn
Hitanemapar með aflestriHitanemapar með aflestri
JárnsmiðstöngJárnsmiðstöng
SuðuhanskarSuðuhanskar
3

Clean and taper

Brush off all the scale, then file a long taper on the first 3 cm so it passes the first hole.

Nauðsynleg verkfæri:

VírburstasettVírburstasett
ÞjalasettÞjalasett
SkrúfstykkiSkrúfstykki
4

Wax and draw

Clamp the drawplate in the vise. Wax the rod, push the taper through the first hole it does not slip through, and pull straight out with the draw tongs in one steady pull.

Efni fyrir þetta skref:

BýflugnavaxBýflugnavax20 g

Nauðsynleg verkfæri:

Dráttarplata úr stáliDráttarplata úr stáli
DráttartöngDráttartöng
SkrúfstykkiSkrúfstykki
Vinnuhanskar úr leðriVinnuhanskar úr leðri
5

Anneal every two holes

Draw through each next hole without skipping. After every two holes, coil the wire and anneal it again: hold it at 793 °C (1460 °F) for 30 minutes, cool in the oven no faster than 500 °C an hour to 682 °C (1260 °F), then cool in air.

Efni fyrir þetta skref:

BýflugnavaxBýflugnavax1 stykki

Nauðsynleg verkfæri:

Dráttarplata úr stáliDráttarplata úr stáli
DráttartöngDráttartöng
HitameðferðarofnHitameðferðarofn
Hitanemapar með aflestriHitanemapar með aflestri
6

Finish soft

Stop at the diameter your balls need, checked with the caliper, and give the coil a last anneal so it is soft for heading.

Nauðsynleg verkfæri:

Stafrænn skífmælir 6 tommurStafrænn skífmælir 6 tommur
HitameðferðarofnHitameðferðarofn
Hitanemapar með aflestriHitanemapar með aflestri
7

Troubleshooting

Bearing steel wire troubleshooting.

Flow

Loading...

Efni

3

Nauðsynleg verkfæri

15

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...