Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)
Charlie

Búin til af

Charlie

4. nóvember 2026DE
6
0
0
0
0

Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)

The old way of getting bismuth from ore that holds it as the metal: heat the lumps just enough in sloping iron tubes and the bismuth, which melts easily, runs out of the rock into pots under charcoal. It takes 30-60 minutes a charge but gets only about two-thirds of the metal. Not given: the furnace temperature. Source: E. Thorpe, Dictionary of Applied Chemistry vol. I (1912), Bismuth, p. 458. Picture: Thorpe's Fig. 1, the furnace in plan.
Miðlungs
30-60 minutes per charge

Leiðbeiningar

1

Pick and break the ore

Sort the ore (7-12 % bismuth) by hand from the waste rock as far as possible and break it into pieces the size of a hazel nut.

Efni fyrir þetta skref:

Hreint bismútgrýtiHreint bismútgrýti1 12 cwt per tube charge

Nauðsynleg verkfæri:

HamarHamar
IðnaðarplötuvogIðnaðarplötuvog
2

Charge the tubes

Load about 12 cwt into each inclined iron tube of the furnace, leaving room to stir from the upper end. Close the upper ends with iron plates and the lower ends with plates pierced with round holes. Under each lower end stand an iron pot holding powdered charcoal, kept gently warm by a small charcoal fire.

Efni fyrir þetta skref:

ViðarkolViðarkol1 powdered, in the pots and for the pot fire

Nauðsynleg verkfæri:

BismútbræðsluofnBismútbræðsluofn
JárndeiglaJárndeigla
3

Sweat out the bismuth

Fire the furnace with wood so that the metal flows easily. In about 10 minutes the bismuth begins to run into the pots, where the charcoal covers it from the air. Stir the ore now and then with an iron rod from the upper end; in 30-60 minutes the charge is done. 20 cwt of ore burns about 63 cubic feet of wood.

Efni fyrir þetta skref:

EldiviðurEldiviður1 about 63 cu ft per 20 cwt of ore

Nauðsynleg verkfæri:

BismútbræðsluofnBismútbræðsluofn
JárnteinnJárnteinn
4

Rake out and recharge

Rake the spent ore (bismuth barley) out of the upper end into the tank and refill at once with fresh ore.

Nauðsynleg verkfæri:

JárnhrífaJárnhrífa
BismútbræðsluofnBismútbræðsluofn
5

Cast ingots

Ladle the bismuth from the pots into moulds and cast ingots of 25-50 lb.

Nauðsynleg verkfæri:

JárndeiglaJárndeigla
SteypuskálSteypuskál
StangamótStangamót

Efni

3
  • 1 12 cwt per tube charge
    Staðgengill
  • 1 powdered, in the pots and for the pot fire
    Staðgengill
  • 1 about 63 cu ft per 20 cwt of ore
    Staðgengill

Nauðsynleg verkfæri

8

Þessi teikning býr til

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...