Carbon Resistance Element: Lampblack in Alkyd and Chinese Wood Oil on Laminated Phenolic
A carbon resistance film for radio sets. Chicago Telephone Supply's Cooper (US 2,120,930, 1938) found that lampblack bound in phenolic resin kept drifting, so he bound it in alkyd resin modified with Chinese wood oil (tung oil). Sprayed on laminated phenolic and baked up to 165 °C, the film becomes insoluble and holds its value in heat and damp. His mix gave about 50,000 ohms in an element of ordinary size, with a film about 0.003 inch thick.
The picture: our diagram.
Miðlungs
1 day
Leiðbeiningar
1
1
Make the binder: 72 alkyd, 28 wood oil
Make the binder: 72 alkyd, 28 wood oil
Mix 72 parts of alkyd resin with 28 parts of Chinese wood oil (tung oil).
Efni fyrir þetta skref:
Glyptal-alkýðkvoða72 parts
Tungolía28 partsNauðsynleg verkfæri:
Skálavog
Glerbikar
Hrærari
Gúmmíhanskar2
2
Mix 25 binder, 14 lampblack, 61 solvent
Mix 25 binder, 14 lampblack, 61 solvent
Thoroughly mix 25 parts of the binder with 14 parts of lampblack and 61 parts of a solvent for the binder. The patent does not name the solvent. Ours: xylene.
Efni fyrir þetta skref:
Lampasót14 partsNauðsynleg verkfæri:
Xýlen
Skálavog
Glerbikar
Hrærari
Heilgríma
Gúmmíhanskar3
3
Spray onto laminated phenolic
Spray onto laminated phenolic
Spray the mixture as a thin film onto a base of laminated phenolic. The patent's film is about 0.003 inch thick.
Efni fyrir þetta skref:
Samsett plata úr fenólplastefni1 stykkiNauðsynleg verkfæri:
Sprautubyssa
Loftþjappa
Heilgríma
Gúmmíhanskar4
4
Bake: 40 °C up to 165 °C, hold 1 hour
Bake: 40 °C up to 165 °C, hold 1 hour
Put it in an oven at about 40 °C, raise the heat gradually over one hour to 165 °C and hold there one more hour. Take it out and let it cool; it is ready for use.
Nauðsynleg verkfæri:
Þurrkofn
Ofnhitamælir
Hitaþolnir hanskarEfni
4- 72 partsStaðgengill
- 28 partsStaðgengill
- 14 partsStaðgengill
- 1 stykkiStaðgengill
Nauðsynleg verkfæri
11- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Loftþjappa3% þóknunMagento Legacy Storeships internationallyStaðgengill
- Staðgengill
- Staðgengill
- Staðgengill
Þessi teikning býr til
Tengd Blueprint
Þessi blueprint deila þekkingu — tækni, efni eða meginreglur

Glyptal Resin from Glycerin and Phthalic Anhydride: Callahan, 1914
eftir Charlie
Lífrænt
20
0
0
0
0
0

Tung Oil Pressed from the Seeds of Tung Nuts
eftir Mary
Trésmiði
10
0
0
0
0
0

Making Lampblack Pigment — Collecting Carbon Soot from a Burning Flame
eftir Charlie
LIST
186
0
0
0
6
0

Hættulegt
Laminated Phenolic Paper Sheet: Bakelite-Coated Kraft Paper Hot-Pressed and Baked (O'Conor, Westinghouse 1918)
eftir Charlie
Iðnaður
3
0
0
0
0
0
CC0 opinbert ríki
Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.
Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.