Electrolytic Iron: Brown Ferrous Electrolyte, Rotating Cathode at 75-77 °C, Graphite Anodes (Bouchayer, US 1,516,326)
Charlie

Búin til af

Charlie

31. október 2026DE
0
0
0
0
0

Electrolytic Iron: Brown Ferrous Electrolyte, Rotating Cathode at 75-77 °C, Graphite Anodes (Bouchayer, US 1,516,326)

Iron plated out of a fresh green ferrous bath comes off rough and useless. Bouchayer first stirred the bath in air until it turned bright brown; the iron oxychloride formed takes care of the hydrogen at the cathode, and the deposit grows even and compact at high current. Result: electrolytic iron, deposited at about 98 % current yield. Source: Bouchayer, US 1,516,326 (1924). Not given: cathode material, purity of the iron. Picture drawn by Youblob.
Lengra kominn
Factory process

Leiðbeiningar

1

Make up the electrolyte at 20 °Bé

Dissolve ferrous sulfate in water (Bouchayer also allows ferrous chloride or a mix). Concentration: e.g. 20 °Bé, then keep it constant.

Efni fyrir þetta skref:

JárnsúlfatJárnsúlfat1 as required

Nauðsynleg verkfæri:

VatnVatn
FlotvogFlotvog
RafgreiningarkerRafgreiningarker
2

Stir it in air until brown

Agitate the green bath in air, e.g. by turning the anode, until it is bright brown and stops foaming. Used green, it gives only an irregular deposit.

Nauðsynleg verkfæri:

RafgreiningarkerRafgreiningarker
3

Circulate it through iron filings

Pump the electrolyte through a mass of iron filings in a separate vessel; it takes back iron and forms the ferric hydroxide that keeps the bath working. Keep it moving fast past the anodes: this lowers the phosphorus.

Efni fyrir þetta skref:

JárnspænirJárnspænir1 as required

Nauðsynleg verkfæri:

VatnsdælaVatnsdæla
4

Deposit on a rotating cathode

Electrolyse between graphite anodes and a rotating cathode. Temperature: e.g. 75-77 °C at 1000 A/m², held exactly constant and below boiling; cathode speed: e.g. 120 m/min at 800 A/m². Cathode material: not given.

Nauðsynleg verkfæri:

GrafítskautGrafítskaut
JafnstraumsgjafiJafnstraumsgjafi
HitamælirHitamælir
RafgreiningarkerRafgreiningarker
5

Strip and reheat the deposit

Take the compact iron deposit off the cathode; it is usable after a slight reheating (temperature not given).

Nauðsynleg verkfæri:

RafgreiningarkerRafgreiningarker

Efni

2
  • 1 as required
    Staðgengill
  • 1 as required
    Staðgengill

Nauðsynleg verkfæri

7

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...