Fired Silver Paint: Precipitated Silver and Flux in Polyvinyl Alcohol with Ammonia (Gray, Erie Resistor 1954, Ex. 1)
Ed

Búin til af

Ed

28. október 2026FI
8
0
0
0
0

Fired Silver Paint: Precipitated Silver and Flux in Polyvinyl Alcohol with Ammonia (Gray, Erie Resistor 1954, Ex. 1)

A paint for putting silver electrodes on ceramic, glass or mica. Fine silver powder and a little ceramic flux are held in polyvinyl alcohol dissolved in water, with a trace of ammonia to make the wet paint conduct. So a capacitor can be measured while it is being painted. On firing, the silver becomes a film held on by the flux. The silver settles, so stir while painting. Source: Robert B. Gray, US 2,695,275 (Erie Resistor, 1954), Example 1. Not given: how the silver was precipitated, which flux, the form of the ammonia, and the firing heat. Ours: precipitated silver made by reducing silver chloride with zinc, bismuth subnitrate as the flux (one Gray names), and strong ammonia water. Picture drawn by Youblob.
Byrjandi
1 day

Leiðbeiningar

1

Dissolve 4 g polyvinyl alcohol in the water

For 100 g of paint: dissolve 4 g polyvinyl alcohol in the water, warming it to help it dissolve. The water is the balance, about 35 to 44 g. Warming is ours.

Efni fyrir þetta skref:

PólývínýlalkóhólduftPólývínýlalkóhólduft4 g
Eimað vatnEimað vatn1 as required

Nauðsynleg verkfæri:

SkálavogSkálavog
Bikarglas úr bórsílíkatiBikarglas úr bórsílíkati
HitaplataHitaplata
BórsílíkatglerstöngBórsílíkatglerstöng
2

Grind in 50 g precipitated silver and the flux

Grind 50 g precipitated silver and 2 to 10 g ceramic flux into the solution until smooth. Gray allows some silver chloride left in the silver. Ours: silver from the zinc route, and bismuth subnitrate, one of the fluxes Gray names. The right amount of flux depends on the ceramic.

Efni fyrir þetta skref:

Fellt silfurFellt silfur50 g
Bismút-subnítratBismút-subnítrat1 as required

Nauðsynleg verkfæri:

SkálavogSkálavog
Mortél og mortélstauturMortél og mortélstautur
NítrílhanskarNítrílhanskar
3

Add 0.2 to 1 % ammonia

Stir in ammonia, 0.2 to 1 % of the paint. It evaporates from the film but makes the wet paint conduct. Ours: added as strong ammonia water. Sharp fumes: work in air, goggles.

Efni fyrir þetta skref:

Ammoníaklausn 25-28 %Ammoníaklausn 25-28 %1 as required

Nauðsynleg verkfæri:

BórsílíkatglerstöngBórsílíkatglerstöng
Hlífðargleraugu gegn efnaslettumHlífðargleraugu gegn efnaslettum
NítrílhanskarNítrílhanskar
4

Stir while painting

The silver in this paint settles, so stir it while it is being applied.

Nauðsynleg verkfæri:

BórsílíkatglerstöngBórsílíkatglerstöng

Efni

5

Nauðsynleg verkfæri

7

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...