Chamois Wash Leather: Frized Pelts Fulled With Fish Oil Eight or Nine Times (Morfit, 1852)
Oil-tawed chamois or wash leather, from Campbell Morfit's Arts of Tanning, Currying and Leather-Dressing (1852): sheep, goat or deer pelts with the grain rubbed off, beaten again and again with fish oil until it is worked right in, warmed so the oil sets in the fibre, then washed of excess oil in weak potash lye and finished soft. No tannin, no alum.
Lengra kominn
About 2 weeks
Leiðbeiningar
1
1
Oil budget
Oil budget
Hleð Jupyter-vinnubók…
2
2
Read The Arts of Tanning
Read The Arts of Tanning
"Oiled leather is commonly known as chamois, or wash-leather ... from its property of bearing wetting and washing."
3
3
Make pelts and friz
Make pelts and friz
Choose the finest goat, sheep, lamb or deer skins (or thin split sides). Bring them to pelt as for kid leather: wash, lime, fleece, beam and bran. Then friz them: rub with a pumice stone, or work under the round edge of a blunt knife, to remove the grain, even the thickness and soften the skin.
Efni fyrir þetta skref:
Gæra12 stykki
Slökkt kalk1 stykki
Hveitiklíð1 stykkiNauðsynleg verkfæri:
Sútunarker
Skafbeður
Skafhnífur
Vikursteinn4
4
Oil and full
Oil and full
Wring the skins and beat them in the fulling trough until nearly dry. Spread each on the table and sprinkle the grain side with cod or other fish oil, fold them in bundles of four, and beat again 2 to 4 hours. Open and air them briefly, grease again, and full again. Repeat eight or nine times until thoroughly imbued, with no greasy look. 3 to 5 gallons of oil serve a gross of skins. (By hand: beat them in a tub with a heavy wooden mallet, our method.)
Efni fyrir þetta skref:
Fiskilýsi1 stykkiNauðsynleg verkfæri:
Sútunarker
Trésleggja5
5
Warm and set
Warm and set
Hang the skins on hooks from wooden hangers in a warm drying room (his is about 6 ft high and 12 ft square, heated by steam-pipes or a stove). A slight fermentation sets the oil into the fibre.
6
6
Wash out the excess
Wash out the excess
Handle the skins for an hour in slightly warm potash lye of 2 deg Baume, which turns the excess oil to soap. Wring them at the peg, dry, finish on the stretcher and the stake (horse), and smooth with rollers. For a buff colour dip them in an oak-bark infusion (a dye here, not a tan).
Efni fyrir þetta skref:
Kalíumhýdroxíð1 stykki
Eikarbörkur (mulinn)1 stykkiNauðsynleg verkfæri:
Sútunarker
20 lítra fata7
7
Troubleshooting
Troubleshooting
Chamois troubleshooting.
Flow
Loading...
8
8
History and honest limits
History and honest limits
From Campbell Morfit, **The Arts of Tanning, Currying, and Leather-Dressing** (1852), "Oiled Leather" (checked on the archive.org scan artsoftanningcur00morf, pp. 433-436). He refers back to kid leather for the pelt stage. Hand fulling, the tools and the diagram are ours.
Efni
6- 12 stykkiStaðgengill
- 1 stykkiStaðgengill
- 1 stykkiStaðgengill
- 1 stykkiStaðgengill
- 1 stykkiStaðgengill
- 1 stykkiStaðgengill
Nauðsynleg verkfæri
6- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
Þessi teikning býr til
Tengd Blueprint
Þessi blueprint deila þekkingu — tækni, efni eða meginreglur
CC0 opinbert ríki
Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.
Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.